Importance of Wear Evaluation on DLC in Humidity
Diamond-like carbon (DLC) coatings possess enhanced tribological properties, namely excellent wear resistance and a very low coefficient of friction (COF). DLC coatings impart diamond characteristics when deposited on different materials. Favorable tribo-mechanical properties make DLC coatings preferable in various industrial applications, such as aerospace parts, razor blades, metal cutting tools, bearings, motorcycle engines, and medical implants.
DLC coatings exhibit very low COF (below 0.1) against steel balls under high vacuum and dry conditions12. However, DLC coatings are sensitive to environmental condition changes, particularly relative humidity (RH)3. Environments with high humidity and oxygen concentration may lead to significant increase in COF4. Reliable wear evaluation in controlled humidity simulates realistic environmental conditions of DLC coatings for tribological applications. Users select the best DLC coatings for target applications with proper comparison
of DLC wear behaviors exposed to different humidity.
Measurement Objective
This study showcases the Nanovea Tribometer equipped with a humidity controller is the ideal tool for investigating wear behavior of DLC coatings at various relative humidity.
Test Procedure
Friction and wear resistance of DLC coatings were evaluated by the Nanovea Tribometer. Test parameters are summarized in Table 1. A humidity controller attached to the tribo-chamber precisely controlled the relative humidity (RH) with an accuracy of ±1%. Wear tracks on DLC coatings and wear scars on SiN balls were examined using an optical microscope after tests.
Note: Any solid ball material can be applied to simulate the performance of different material coupling under environmental conditions such as in lubricant or high temperature.
Results and Discussion
DLC coatings are great for tribological applications due to their low friction and superior wear resistance. The DLC coating friction exhibits humidity dependent behavior shown in Figure 2. The DLC coating shows a very low COF of ~0.05 throughout the wear test in relatively dry conditions (10% RH). The DLC coating exhibits a constant COF of ~0.1 during the test as RH increases to 30%. The initial run-in stage of COF is observed in the first 2000 revolutions when RH rises above 50%. The DLC coating shows a maximum COF of ~0.20, ~0.26 and ~0.33 in RH of 50, 70 and 90%, respectively. Following the run-in period, the DLC coating COF stays constant at ~0.11, 0.13 and 0.20 in RH of 50, 70 and 90%, respectively.
Figure 3 compares SiN ball wear scars and Figure 4 compares DLC coating wear tracks after the wear tests. The diameter of the wear scar was smaller when the DLC coating was exposed to an environment with low humidity. Transfer DLC layer accumulates on the SiN ball surface during the repetitive sliding process at the contact surface. At this stage, the DLC coating slides against its own transfer layer which acts as an efficient lubricant to facilitate the relative motion and restrain further mass loss caused by shear deformation. A transfer film is observed in the wear scar of the SiN ball in low RH environments (e.g. 10% and 30%), resulting in a decelerated wear process on the ball. This wear process reflects on the DLC coating’s wear track morphology as shown in Figure 4. The DLC coating exhibits a smaller wear track in dry environments, due to the formation of a stable DLC transfer film at the contact interface which significantly reduces friction and wear rate.
Conclusion
Humidity plays a vital role in the tribological performance of DLC coatings. The DLC coating possesses significantly enhanced wear resistance and superior low friction in dry conditions due to the formation of a stable graphitic layer transferred onto the sliding counterpart (a SiN ball in this study). The DLC coating slides against its own transfer layer, which acts as an efficient lubricant to facilitate the relative motion and restrain further mass loss caused by shear deformation. A film is not observed on the SiN ball with increasing relative humidity, leading to an increased wear rate on the SiN ball and the DLC coating.
The Nanovea Tribometer offers repeatable wear and friction testing using ISO and ASTM compliant rotative and linear modes, with optional humidity modules available in one pre- integrated system. It allows users to simulate the work environment at different humidity, providing users an ideal tool to quantitatively assess the tribological behaviors of materials under different work conditions.
Learn More about the Nanovea Tribometer and Lab Service
1 C. Donnet, Surf. Coat. Technol. 100–101 (1998) 180.
2 K. Miyoshi, B. Pohlchuck, K.W. Street, J.S. Zabinski, J.H. Sanders, A.A. Voevodin, R.L.C. Wu, Wear 225–229 (1999) 65.
3 R. Gilmore, R. Hauert, Surf. Coat. Technol. 133–134 (2000) 437.
4 R. Memming, H.J. Tolle, P.E. Wierenga, Thin Solid Coatings 143 (1986) 31
Categories
- Application Notes
- Block on Ring Tribology
- Corrosion Tribology
- Friction Testing | Coefficient of Friction
- High Temperature Mechanical Testing
- High Temperature Tribology
- Humidity and Gases Tribology
- Humidity Mechanical Testing
- Indentation | Creep and Relaxation
- Indentation | Fracture Toughness
- Indentation | Hardness and Elastic
- Indentation | Loss and Storage
- Indentation | Stress vs Strain
- Indentation | Yield Strength and Fatigue
- Laboratory Testing
- Linear Tribology
- Liquid Mechanical Testing
- Liquid Tribology
- Low Temperature Tribology
- Mechanical Testing
- Press Release
- Profilometry | Flatness and Warpage
- Profilometry | Geometry and Shape
- Profilometry | Roughness and Finish
- Profilometry | Step Height and Thickness
- Profilometry | Texture and Grain
- Profilometry | Volume and Area
- Profilometry Testing
- Ring on Ring Tribology
- Rotational Tribology
- Scratch Testing | Adhesive Failure
- Scratch Testing | Cohesive Failure
- Scratch Testing | Multi-Pass Wear
- Scratch Testing | Scratch Hardness
- Scratch Testing Tribology
- Tribology Testing
- Uncategorized
Archives
- August 2026
- June 2026
- May 2026
- March 2026
- November 2025
- September 2023
- August 2023
- June 2023
- May 2023
- July 2022
- May 2022
- April 2022
- January 2022
- December 2021
- November 2021
- October 2021
- September 2021
- August 2021
- July 2021
- June 2021
- May 2021
- March 2021
- February 2021
- December 2020
- November 2020
- October 2020
- September 2020
- July 2020
- May 2020
- April 2020
- March 2020
- February 2020
- January 2020
- November 2019
- October 2019
- September 2019
- August 2019
- July 2019
- June 2019
- May 2019
- April 2019
- March 2019
- January 2019
- December 2018
- November 2018
- October 2018
- September 2018
- July 2018
- June 2018
- April 2018
- March 2018
- February 2018
- November 2017
- October 2017
- September 2017
- August 2017
- June 2017
- May 2017
- March 2017
- February 2017
- January 2017
- November 2016
- October 2016
- August 2016
- July 2016
- June 2016
- May 2016
- April 2016
- March 2016
- February 2016
- January 2016
- December 2015
- November 2015
- October 2015
- September 2015
- August 2015
- July 2015
- June 2015
- May 2015
- April 2015
- March 2015
- February 2015
- January 2015
- November 2014
- October 2014
- September 2014
- August 2014
- July 2014
- June 2014
- May 2014
- April 2014
- March 2014
- February 2014
- January 2014
- December 2013
- November 2013
- October 2013
- September 2013
- August 2013
- July 2013
- June 2013
- May 2013
- April 2013
- March 2013
- February 2013
- January 2013
- December 2012
- November 2012
- October 2012
- September 2012
- August 2012
- July 2012
- June 2012
- May 2012
- April 2012
- March 2012
- February 2012
- January 2012
- December 2011
- November 2011
- October 2011
- September 2011
- August 2011
- July 2011
- June 2011
- May 2011
- November 2010
- January 2010
- April 2009
- March 2009
- January 2009
- December 2008
- October 2008
- August 2007
- July 2006
- March 2006
- January 2005
- April 2004