EE.UU./GLOBAL: +1-949-461-9292
EUROPA: +39-011-3052-794
CONTACTO

Categoría: Pruebas de perfilometría

 

Soft and transparent materials including a biomedical membrane, microfluidic device, and wearable sensor for non-contact profilometry applications

Non-Contact Profilometry of Soft and Transparent Materials

Application Note | Non-Contact 3D Profilometry

Non-Contact Profilometry of Soft and Transparent Materials

Comprehensive Characterization of Challenging Surfaces Without Contact, Deformation, or Sample Preparation

Examples of soft and transparent material applications for non-contact profilometry, including biomedical membranes, microfluidics, and wearable sensors

Research & Experimental Testing

Craig Leising

Visual Design & Editorial

Andrew Shore

Introducción

Soft, transparent, and easily deformable materials are increasingly important across advanced applications including flexible bioelectronics, wearable sensors, biomedical interfaces, microfluidic devices, and other polymer-based technologies. Characterizing these materials can be difficult because the measurement method itself may influence the surface or fail to capture it reliably.

Contact-based techniques can deform, scratch, or move soft materials during measurement, while transparent or absorptive surfaces can present additional challenges for some optical techniques. Non-contact profilometry avoids physical interaction with the sample while enabling quantitative surface characterization across challenging material types.

In this study, an extremely soft and translucent petroleum-jelly-based material was selected as a demanding proof-of-concept sample. Using the NANOVEA ST400 Profilometer, the surface was characterized without physical contact or sample preparation to demonstrate the broader capability of non-contact profilometry for delicate and difficult-to-measure materials.

The Advantage of Non-Contact Profilometry for Challenging Materials

Soft materials can be difficult to measure accurately because physical contact may alter the surface during the measurement itself. Films, gels, and other compliant materials can deform, scratch, or move under a contacting probe, potentially changing the geometry being characterized.

Transparent and absorptive surfaces can introduce additional measurement challenges for some optical techniques, including effects associated with light transmission, absorption, and internal reflections. NANOVEA Non-Contact Profilometers use axial chromatism to determine surface height without physically contacting the sample.

This combination enables quantitative characterization of challenging surfaces while minimizing measurement influence. Depending on the application, measurements can include surface roughness, flatness, 3D topography, surface area, profile geometry, and other dimensional characteristics without requiring sample preparation.

Objetivo de medición

The objective of this study was to demonstrate non-contact surface characterization on an extremely soft and translucent material, representing the type of measurement challenge encountered when a surface may be altered by physical contact or prove difficult for some optical techniques.

A petroleum-jelly-based lip balm was selected as a deliberately challenging proof-of-concept sample because of its softness and translucency. The sample was measured using the NANOVEA ST400 Profilometer without physical contact or sample preparation.

The resulting measurement was used to obtain 3D topography, 2D profile data, surface roughness, flatness, and 3D surface area, demonstrating the range of quantitative surface information that can be obtained from a delicate material using non-contact profilometry.

NANOVEA ST400 Non-Contact

Perfilómetro óptico

Optical Profilometry Results

Soft transparent petroleum-jelly-based lip balm sample used for non-contact profilometry

Soft, translucent petroleum-jelly-based sample used for non-contact profilometry.

Soft transparent petroleum-jelly-based sample positioned under the NANOVEA ST400 profilometer for non-contact surface measurement

The sample being scanned by the NANOVEA ST400 for non-contact surface measurement.

3D Profile Measurement

The NANOVEA ST400 captured the 3D surface of the extremely soft and translucent sample without physically contacting the material. The resulting topography was used to evaluate multiple aspects of the surface, including ISO 25178 surface parameters, 3D surface area, and flatness corresponding to ISO 12781. A 2D cross-section was also extracted from the measurement to provide additional profile detail.

Obtaining these measurements from such a soft and translucent surface demonstrates the value of non-contact profilometry for materials that could otherwise be altered by a contacting probe or present challenges for some optical techniques. Quantitative surface geometry can be acquired while preserving the condition of the measured surface.

3D non-contact profilometry measurement of a soft transparent petroleum-jelly-based sample with ISO 25178 surface parameters

3D surface profile of the soft, transparent sample with ISO 25178 surface parameters and flatness analysis.

2D Profile Measurement

2D profile extracted from non-contact profilometry of a soft transparent petroleum-jelly-based sample

2D profile extracted from the non-contact 3D surface measurement across a 4 mm section of the sample.

An intensity/contrast image was also acquired simultaneously with the 3D surface measurement, providing complementary visual information alongside the measured topography.

False-color height map from non-contact profilometry of a soft transparent petroleum-jelly-based sample

False-color height map showing surface height variation across the soft, translucent sample.

Intensity image acquired during non-contact profilometry of a soft transparent petroleum-jelly-based sample

Intensity image acquired simultaneously with the 3D surface measurement.

Conclusión

This study demonstrates how non-contact profilometry can characterize surfaces that combine two particularly difficult measurement conditions: extreme softness and translucency. Using the NANOVEA ST400, quantitative 3D surface data were acquired without physically contacting or preparing the sample.

A petroleum-jelly-based lip balm was selected as a deliberately challenging proof-of-concept material rather than as the end application itself. Its soft, translucent surface provided a practical demonstration of the ability to obtain surface roughness, flatness, 3D surface area, profile geometry, and complementary intensity data while minimizing the influence of the measurement process on the surface.

This capability is relevant wherever delicate, compliant, transparent, or absorptive materials must be characterized without deformation or surface damage. As soft polymers, gels, transparent elastomers, and related materials continue to appear in areas such as biomedical interfaces, wearable technologies, microfluidics, and advanced polymer systems, non-contact surface measurement provides a useful approach for evaluating their surface geometry and topography.

Frequently Asked Questions About Non-Contact Profilometry

Why is non-contact profilometry useful for soft materials?

Soft materials can deform, scratch, or move when touched by a contacting probe. Non-contact profilometry measures the surface optically, reducing the risk that the measurement itself alters the geometry being characterized.

Can non-contact profilometry measure transparent materials?

Yes, depending on the optical technology and material. NANOVEA profilometers use axial chromatism to determine surface height and can characterize transparent, opaque, specular, diffusive, polished, and rough surfaces without physical contact.

Can soft and transparent surfaces be measured without sample preparation?

In this study, the soft and transparent petroleum-jelly-based sample was measured without sample preparation. Avoiding coatings or other surface modification can be especially valuable when the original surface condition needs to be preserved.

What can be measured with non-contact 3D profilometry?

Non-contact 3D profilometry can provide quantitative measurements including surface roughness, 3D topography, flatness, surface area, 2D profiles, and other dimensional characteristics, depending on the measurement objective and surface geometry.

What types of materials benefit from non-contact surface measurement?

Non-contact measurement is especially useful for materials that are soft, delicate, transparent, semi-transparent, easily scratched, or otherwise difficult to probe physically. It can also be useful when maintaining the original surface condition is important.

How is non-contact profilometry different from contact profilometry?

Contact profilometry uses a physical stylus that moves across the surface. Non-contact profilometry acquires surface height optically, eliminating probe-to-sample contact and reducing the possibility of contact-induced deformation, scratching, or movement on sensitive materials.

Pacemaker and endocardial pacing leads shown in a translucent medical illustration for pacing lead insulation wear testing

Pacing Lead Insulation Wear Testing in Hanks’ Solution

Application Note | Medical Device Tribology

Nano-Friction and Wear Testing of Pacing Lead Insulation in Hanks’ Solution

Tribological analysis of silicone and polyether-polyurethane endocardial lead materials

Medical illustration of a pacemaker with two endocardial pacing leads routed into the heart for pacing lead insulation wear testing context

Research & Experimental Testing

Doctor Duanjie Li

Visual Design & Editorial

Andrew Shore

Introducción

A pacemaker is a medical device used to regulate heart rhythm and maintain an adequate heart rate. It is typically implanted in the chest or abdomen and sends electrical impulses to the heart muscle through endocardial pacing leads.

As pacemakers remain a widely used treatment for cardiac rhythm disorders, the quality and service life of pacing leads are critical to long-term device performance. Lead failures can create serious risks for patients and may require surgical replacement, making pacing lead insulation wear testing an important part of material evaluation for implantable cardiac devices.1–5
Endocardial pacing leads with insulated lead bodies used in implantable cardiac devices

Endocardial pacing leads transmit electrical impulses from a pacemaker to the heart while operating in a dynamic body-fluid environment.

Why Friction and Wear Matter for Endocardial Lead Insulation

The outer insulation material of an endocardial lead requires several key properties, including biological inertness, high flexibility, fracture toughness, and long service life. Low friction can reduce interaction between the lead and the blood vessel, helping minimize vessel irritation during implantation and movement.

Wear resistance is also critical. Endocardial leads experience continuous movement from the heart and surrounding body structures, while operating in a body-fluid environment that can influence friction, wear, and material response.

Because of this complex environment, endocardial lead insulation should be evaluated using controlled tribological methods that simulate relevant contact conditions. Testing in Hanks’ solution allows the friction and wear behavior of lead insulation materials to be compared under a simulated body-fluid condition rather than relying only on dry testing.

Nano-friction test setup for measuring pacing lead insulation materials in Hanks’ solution

Nano-friction test setup used to evaluate endocardial pacing lead insulation materials under low-load contact conditions.

Objetivo de medición

This study compares the nano-friction and wear behavior of endocardial pacing lead insulation materials in Hanks’ solution. Silicone and polyether-polyurethane lead materials were evaluated to determine how each material responds under simulated body-fluid conditions.

Low-load nano-friction testing was performed using the Nano Module of the Probador mecánico NANOVEA to measure coefficient of friction at controlled contact force. Reciprocating wear testing was then performed using a NANOVEA Tribometer to compare wear resistance under linear sliding contact.

NANOVEA T50 Compacto
Tribómetro de peso libre

NANOVEA PB1000 Plataforma grande Comprobador mecánico

Measurement Principle

Nano-Friction Measurement Principle

Nano-friction testing measures the coefficient of friction (COF) between the test surface and a controlled counter material under very low applied load. In this study, the indenter made contact with the pacing lead insulation surface while the Nano Module maintained a constant load throughout the measurement.

The Nano Module uses a fast piezoelectric system and load cell to adjust the ball position and keep the applied load stable during sliding. The sample is moved at a controlled speed while lateral force is measured and plotted against displacement.

A stainless steel ball with a 6 mm diameter is commonly used for this type of measurement, although other counter materials, shapes, and sizes can be selected to simulate different contact conditions. This allows pacing lead insulation materials to be evaluated under controlled low-load friction conditions relevant to biomedical device applications.

Schematic of the nano-friction measurement principle showing a ball-tip indenter under controlled constant load, a capacitive depth sensor, non-destructive load, and reciprocating sample motion on a friction spring table

Nano-friction measurement schematic showing controlled low-load sliding contact and lateral force measurement during reciprocating motion.

Reciprocating Wear Principle

Reciprocating wear testing evaluates material response under repeated linear sliding contact. A flat or spherical counter material is loaded against the test sample with a precisely known force, while the sample moves back and forth in a controlled reciprocating motion.

The counter material, such as a pin or ball, is mounted on a stiff lever that functions as a low-friction force transducer. As the sample moves, frictional forces between the counter material and the sample are measured using a strain gauge sensor on the tribometer arm.

After the test, the resulting wear track can be examined to compare material damage, wear scar geometry, and surface response. This method allows friction and wear behavior to be studied under controlled conditions, including variations in time, contact pressure, sliding speed, temperature, humidity, and lubrication environment.

Schematic of the reciprocating wear principle showing adjustable weights, tribometer arm, pin or ball holder, strain gauge, sample stage, linear wear track, and linear reciprocating motion

Linear reciprocating wear schematic showing a pin or ball counterface sliding across the sample to generate a wear track under controlled load.

Procedimiento de ensayo

The coefficient of friction (COF) of the pacing lead materials was measured against a stainless steel 440 ball with a 6 mm diameter. Testing was performed using the Nano Module of the Nanovea Mechanical Tester.

The sample was immersed in Hanks’ solution to simulate a body-fluid environment. A low applied load of 50 mN was maintained throughout the test, while the ball slid against the lead surface at a constant speed of 20 mm/min over a total sliding distance of 10 mm.

Wear resistance was evaluated using a Nanovea Tribometer with the Linear Reciprocating Wear Module. During the wear test, a stainless steel 303 block measuring 10 × 10 mm² was used as the counter material, and the coefficient of friction was recorded in situ at 0.1 s intervals.

After testing, the resulting wear tracks were examined under an optical microscope to compare surface damage on the silicone and polyether-polyurethane lead materials. Stainless steel was used as the counter material in this study; however, custom fixtures and alternative counter materials can be used to simulate specific application conditions.

Parameter Value
Sample Leads made of silicone or polyether-polyurethane (PP)
Normal force 1 N
Velocidad 200 cycles/min
Duration of test 5 h
Environment Hanks’ solution

Wear test parameters used to evaluate silicone and polyether-polyurethane pacing lead materials in Hanks’ solution.

Resultados y debate

Nano-Friction Test

The nano-friction behavior of the silicone and polyether-polyurethane (PP) pacing lead materials was first evaluated using the Nano Module of the Nanovea Mechanical Tester. The coefficient of friction was measured in both dry conditions and Hanks’ solution to compare material response under ambient and simulated body-fluid environments.

Both materials showed significantly lower coefficient of friction in Hanks’ solution than under dry conditions. In Hanks’ solution, the silicone lead exhibited a COF of approximately 0.15, while the polyether-polyurethane lead exhibited a lower COF of approximately 0.05. Under dry conditions, the values were substantially higher, at approximately 0.6 for silicone and 0.5 for polyether-polyurethane.

These results demonstrate the importance of testing pacing lead insulation materials under application-relevant environmental conditions. Hanks’ solution had a strong effect on the measured friction behavior, showing that dry testing alone may not represent the tribological response of lead insulation materials in a simulated body-fluid environment.

The low-load control of the Nano Module allowed the applied force to remain constant at 50 mN during the measurement. This enabled controlled simulation of low-contact-force interaction between the lead material and surrounding biological structures.

Graph comparing coefficient of friction of silicone and polyether-polyurethane pacing lead materials in dry conditions and Hanks’ solution

Coefficient of friction comparison for silicone and polyether-polyurethane pacing lead materials in dry conditions and Hanks’ solution.

Wear Test

Wear resistance was evaluated using a Nanovea Tribometer to compare the silicone and polyether-polyurethane pacing lead materials in Hanks’ solution. After testing, the lead surfaces were examined visually and under optical microscopy to compare the extent of wear damage.

The silicone lead showed a large wear scar with a width of approximately 1.2 mm. Microscopic observation indicated severe wear on the silicone lead, with parallel deep grooves formed along the movement direction of the rubbing block.

In comparison, the polyether-polyurethane lead showed a narrower wear scar of approximately 0.6 mm. The observed wear was milder, with only several small scratches visible on the shallow surface.

Wear of the lead outer insulation can contribute to pacing and sensing abnormalities, making wear resistance an important factor in endocardial lead material selection.6 These results indicate that polyether-polyurethane provided lower friction and better wear resistance than silicone under the tested conditions.

Before-and-after wear comparison of silicone and polyether-polyurethane pacing lead surfaces, including 400x microscope images showing more severe wear on silicone and milder wear on polyether-polyurethane.

Silicone pacing lead surface before wear testing in Hanks’ solution

Silicone pacing lead surface before reciprocating wear testing.

Polyether-polyurethane pacing lead surface before wear testing in Hanks’ solution

Polyether-polyurethane pacing lead surface before reciprocating wear testing.

Silicone pacing lead surface after wear testing showing a large wear scar

Silicone pacing lead surface after wear testing, showing a pronounced wear scar.

Polyether-polyurethane pacing lead surface after wear testing showing a smaller wear scar

Polyether-polyurethane pacing lead surface after reciprocating wear testing.

Microscope image at 400x magnification showing severe wear grooves on silicone pacing lead surface

400x microscope image of the silicone pacing lead after wear testing, showing deep parallel wear grooves.

Microscope image at 400x magnification showing mild wear on polyether-polyurethane pacing lead surface

400x microscope image of the polyether-polyurethane pacing lead after wear testing, showing comparatively mild surface wear.

Conclusión

This study demonstrated the use of low-load nano-friction testing and reciprocating wear testing to evaluate endocardial pacing lead insulation materials in Hanks’ solution. The Nano Module of the NANOVEA Mechanical Tester measured coefficient of friction under controlled low-load contact, while the NANOVEA Tribometer simulated wear behavior under reciprocating sliding motion.

Testing in Hanks’ solution showed a clear difference between silicone and polyether-polyurethane lead materials. Polyether-polyurethane exhibited lower coefficient of friction and better wear resistance than silicone under the tested conditions, making it the stronger candidate for the outer insulation material of endocardial pacing leads in this study.

These results highlight the importance of evaluating biomedical materials under application-relevant environments rather than relying only on dry testing. Controlled nano-friction and tribology testing can help compare candidate materials, quantify friction response, and evaluate wear resistance for implantable medical device components.

The NANOVEA Mechanical Tester’s Nano, Micro, and Macro modules operate within a single ISO and ASTM compliant platform, enabling consistent evaluation of hardness, elastic modulus, fracture toughness, and wear from a single system. The NANOVEA Tribometer similarly supports rotative and linear wear modes with optional high-temperature, corrosion, and liquid environment modules.

Referencias

[1] Magney JE, Flynn DM, Parsons JA, Staplin DH, Chin-Purcell MV, Milstein S, Hunter DW. Pacing Clin Electrophysiol. 1993; 16:445–457.
[2] Jacobs DM, Fink AS, Miller RP, Anderson WR, McVenes RD, Lessar JF, Cobian KE, et al. Pacing Clin Electrophysiol. 1993; 16:434–444.
[3] Gupta K, Villareal RP, Rasekh A, Massumi A. Tex Heart Inst J. 2003; 30:84–85.
[4] Magney JE, Parsons JA, Flynn DM, Hunter DW. Pacing Clin Electrophysiol. 1995; 18:1509–1517.
[5] Kazama S, Nishiyama K, Machii M, Tanaka K, Amano T, Nomura T, Ohuchi M, et al. Jpn Heart J. 1993; 34:193–200.
[6] Andrzej K, Barbara M, Agnieszka K, Marcin G. Pacing Clin Electrophysiol. 2013; 36(12):1503–1511.

Frequently Asked Questions About Pacing Lead Insulation Wear Testing

How do you evaluate friction and wear behavior of pacing lead insulation?

Pacing lead insulation can be evaluated using low-load friction testing and reciprocating wear testing. These methods measure coefficient of friction, wear scar formation, and surface damage under controlled load, motion, and environmental conditions.

Why is low-load friction testing important for endocardial leads?

Endocardial leads operate under relatively low contact forces while interacting with blood vessels, tissue, and surrounding structures. Low-load friction testing helps evaluate how insulation materials behave under contact conditions that are closer to the application than high-force mechanical testing alone.

What does coefficient of friction indicate in pacing lead material testing?

Coefficient of friction indicates how much resistance occurs during sliding contact between the lead insulation and a counter material. In this study, lower COF values in Hanks’ solution showed that the test environment had a strong effect on the measured friction behavior of silicone and polyether-polyurethane materials.

Why compare silicone and polyether-polyurethane lead insulation materials?

Silicone and polyether-polyurethane are commonly considered for flexible biomedical insulation applications because they can provide different combinations of flexibility, durability, and surface response. Comparing them under the same test conditions helps identify which material provides lower friction and better wear resistance for the intended application.

Which NANOVEA instruments are used for low-load friction and wear testing?

Low-load coefficient of friction can be measured using the Nano Module of a NANOVEA Mechanical Tester, while reciprocating wear behavior can be evaluated using a NANOVEA Tribometer. Together, these systems allow controlled evaluation of friction, wear, and material response for biomedical components.

How is reciprocating wear testing used for pacing lead materials?

Reciprocating wear testing repeatedly slides a counter material across the sample surface under controlled load to create and evaluate a wear track. For pacing lead insulation materials, this allows comparison of wear scar width, surface damage, and material durability under simulated sliding contact.

Need Reliable Medical Device Friction and Wear Testing?

3D optical profilometry image showing climbing hold surface roughness, pore morphology, and grip-related texture features.

Climbing Hold Surface Roughness Analysis

Application Note | 3D Optical Profilometry

Climbing Hold Surface Roughness Analysis Using 3D Optical Profilometry

Measuring Texture, Porosity, and Topography on Bouldering Holds

Bouldering holds analyzed for climbing hold surface roughness using 3D optical profilometry.

Research & Experimental Testing

Walter Alabiso, PhD

Visual Design & Editorial

Andrew Shore

Introducción

Bouldering is a demanding discipline that combines physical strength, precise body positioning, and an understanding of how the human body interacts with climbing surfaces. On slab routes, where the wall is angled below vertical and positive holds are limited or absent, a climber’s stability depends almost entirely on the tribological interaction between the body and the climbing hold surface.

Climbing hold surface roughness plays a central role in this contact. Roughness provides the microtexture needed for smearing, a technique where high-friction rubber soles are pressed firmly against the surface to expand the effective contact area and generate adherence. A similar mechanism occurs at the fingers, where the ridges of fingerprints and the pliability of skin deform slightly against the hold’s surface features, creating grip through microscopic interlocking.

Porosity contributes to grip performance by absorbing moisture, sweat, or chalk at the contact interface, preventing the formation of a thin lubricating film that would reduce friction. Micro-cracks and surface flaws act as additional friction points, helping the climber maintain lateral tension against the hold surface. Because these features (roughness, porosity, and surface morphology) operate at different scales and interact differently depending on the hold, quantitative 3D surface measurement is essential for comparing how different climbing hold textures perform under real contact conditions.

Bouldering grips used to compare surface roughness, pore morphology, and grip-related topography.

Why Use Non-Contact Profilometry for Climbing Hold Surface Analysis

Climbing holds and rock-like surfaces can include deep pores, steep asperities, sharp valleys, and irregular texture. These features are difficult to measure accurately with contact-based profilometry because a physical stylus can lose contact, deform local surface features, or fail to reach narrow cavities.

NANOVEA’s non-contact optical profilometry uses chromatic light technology to capture surface height data without touching the sample. This makes it suitable for reconstructing complex climbing hold topography, including deep nooks, pores, and surface flaws, while avoiding measurement artifacts caused by local plastic deformation.

Objetivo de medición

The objective of this study was to demonstrate how non-contact 3D optical profilometry can be used to reconstruct and compare the surface roughness, topography, and pore morphology of climbing holds.

Two bouldering grip samples were analyzed: a yellow hold with a smoother, flatter surface and a blue hold with a rougher tactile texture and sharper grip features. The analysis focused on surface height variation, areal roughness parameters, pore coverage, pore size, pore depth, and functional surface behavior.

The NANOVEA JR25 Optical Profilometer measuring the climbing hold samples using an optical sensor.

Measurement Method

El NANOVEA JR25 Optical Profiler was used to measure the yellow and blue bouldering grip samples. Each surface was scanned with a PS4-MG35 single-point optical sensor with an enhanced 3000 µm Z-range, allowing the system to capture deep pores, sharp valleys, and irregular surface texture while maintaining a 4 µm acquisition step in X and Y.

Dual-frequency acquisition was used to reduce light sensor saturation from localized bright spots on the grip surfaces, improving data capture across rough, porous, and uneven areas.

NANOVEA JR25 Portable

Perfilómetro óptico

Test Parameters

Measurement Setting Optical Profilometry Setup
Samples measured Yellow and blue bouldering grip samples
Optical pen PS4-MG35
Z-range 3000 µm
Scan area 5.00 mm × 5.00 mm
X-step size 4.00 µm
Y-step size 4.00 µm
Averaging 1
Measurement type Direct
Acquisition mode Dual frequency
Acquisition rate 100–400 Hz
Light intensity 100%

Optical profilometry test conditions used to measure the bouldering grip samples.

Optical Profilometry Results

Yellow Grip Sample

Surface Roughness Analysis

The 3D rendering below shows the reconstructed surface topography of the yellow climbing grip sample.

3D optical profilometry reconstruction of the yellow climbing grip surface showing pores, roughness, and surface height variation.

A total least-squares plane was removed to study surface properties. The roughness filters S-Gaussian 2.5 µm was applied following ISO 25178 (1/2 cut-off removed at each side). However, the sharp density of pores and asperities and the elevated average roughness make the use of a Gaussian L-filter (8 mm cut off) inapplicable. Therefore, the primary surface was considered, and the roughness parameters are listed in the table below, alongside the 2D false-color map of the filtered surface.

False-color optical profilometry surface roughness map of the yellow climbing grip sample with ISO 25178 height parameters.
ISO 25178-2 – Primary Surface
S-filter (λs): Gaussian, 2.5 µm, 1/2 cut-off
F-operation: [Workflow] Leveled (TLSPL)
Height Parameters
Sq 168.970 µm Altura media cuadrática
Ssk -0.927 Skewness
Código 4.117 Kurtosis
Sp 320.530 µm Altura máxima del pico
Sv 868.116 µm Maximum pit depth
Sz 1188.645 µm Altura máxima
Sa 132.953 µm Altura media aritmética

The average surface roughness Sa is 132.953 µm, whereas the peak-to-valley roughness, Sz amounts to 1188.645 µm. The surface morphology is skewed towards deep valleys (Ssk < 0, Sv > Sp), with a leptokurtotic (Código > 3) distribution of peaks and valleys relative to the average plane.

The following picture shows a 2D photo-simulation of the area under artificial lighting, highlighting the region’s morphology.

2D photo simulation of the yellow climbing grip surface showing pores, roughness, and morphology under artificial lighting.

Pore Morphology Analysis

A pore analysis was performed across the full scanned area using a semi-automated edge-detection algorithm. The analysis identified recessed surface features to quantify pore coverage, pore density, radius, void volume, and maximum depth.

Pore detection analysis of the yellow climbing grip surface using semi-automated edge detection to identify recessed surface features.

The detected pore locations were then mapped across the scanned 5 mm × 5 mm area to evaluate pore coverage, density, and size distribution.

Pore distribution map of the yellow climbing grip sample showing detected recessed surface features across a 5 mm by 5 mm scanned area.
Information
MethodCircle detection
Features detectedPores, recessed objects
Minimum detection diameter0.150 mm
Maximum detection diameter2.000 mm
Number of detected pores206
Surface coverage47.395%
Pore density8.203 particles/mm²
Global Statistics
ParameterUnitMeanStd. Dev.MinMax
Radiusmm0.1270.0490.0760.275
Void volumeµm³4,724,770.7056,748,143.92523,594.1724.422 × 10⁷
Maximum depthµm173.72994.94228.153716.480

Pores covered nearly half of the yellow grip’s scanned surface, with a measured coverage of 47.395% and a pore density of 8.203 particles/mm². The detected pores and cracks were highly heterogeneous in size, volume, and depth, ranging from large crater-like features with a maximum radius of 0.275 mm and void volume above 4.4 × 10⁷ µm³ to smaller pores with a minimum radius of 0.076 mm and void volume of 23,594.172 µm³. This uneven pore distribution is reflected in the large standard deviation measured for void volume and maximum depth.

Functional Surface Parameters (Abbott-Firestone curve)

The Abbott-Firestone curve shows the cumulative areal material distribution of the yellow climbing grip sample. This analysis defines functional surface parameters including Sk, Spk, and Svk according to ISO 25178-2.

Abbott-Firestone curve for the yellow climbing grip sample showing cumulative areal material distribution and functional surface parameters.
Information
Estándar ISO 25178-2
Parameter Value Unit
Sk 409.738 µm
Spk 45.480 µm
Svk 233.446 µm
Smrk1 3.976 %
Smrk2 85.005 %

The chart below shows the peak-valley distribution from the mean plane based on the functional parameters derived from the Abbott-Firestone curve. Valleys are shown in purple, the mean plane in green, and peaks in orange.

Peak-valley distribution map of the yellow climbing grip sample showing valleys, mean plane regions, and peaks derived from Abbott-Firestone functional parameters.
Information
1st threshold Height – c1: 229.209 µm
2nd threshold Height – c2: -180.424 µm
Parameters Unit
Projected area (in %) % 14.995 81.029 3.976
Projected area mm² 3.772 20.381 1.000
Volume of material (in %) % 97.451 48.100 0.973
Volume of material µm³ 1.684 × 10¹⁰ 4.956 × 10⁹ 2.275 × 10⁷

The yellow grip sample shows a dominant mean-plane region with scattered recessed pores and a smaller population of raised peaks. This indicates a surface texture characterized mainly by average-sized pores distributed across the scanned area.

Blue Grip Sample

Surface Roughness Analysis

The 3D rendering below shows the reconstructed surface topography of the blue climbing grip sample.

3D optical profilometry reconstruction of the blue climbing grip surface showing roughness, pores, asperities, and surface height variation.

A total least-squares plane was removed to evaluate the blue grip’s surface properties. An S-Gaussian 2.5 µm roughness filter was applied following ISO 25178, with 1/2 cut-off removed at each side.

Because of the dense pores, asperities, and elevated average roughness, a Gaussian L-filter with an 8 mm cut-off was not applied. The primary surface was used for roughness analysis, with the roughness parameters listed alongside the 2D false-color map of the filtered surface.

False-color optical profilometry surface roughness map of the blue climbing grip sample with ISO 25178 height parameters.
ISO 25178-2 – Primary Surface
S-filter (λs): Gaussian, 2.5 µm, 1/2 cut-off
F-operation: [Workflow] Leveled (TLSPL)
Height Parameters
Sq 211.440 µm Altura media cuadrática
Ssk -0.682 Skewness
Código 3.672 Kurtosis
Sp 522.404 µm Altura máxima del pico
Sv 720.164 µm Maximum pit depth
Sz 1242.568 µm Altura máxima
Sa 166.719 µm Altura media aritmética

The blue grip sample had an average surface roughness, Sa, of 166.719 µm and a peak-to-valley roughness, Sz, of 1242.568 µm. The negative skewness value, Ssk &lt; 0, indicates that the surface morphology is skewed toward deep valleys, while Sv &gt; Sp shows that the maximum pit depth exceeded the maximum peak height.

The kurtosis value, Sku &gt; 3, indicates a leptokurtotic height distribution, meaning the blue grip surface contains sharper or more extreme peaks and valleys relative to the average plane.

The 2D photo simulation below highlights the blue climbing grip’s surface morphology under artificial lighting.

2D photo simulation of the blue climbing grip surface showing pores, roughness, and morphology under artificial lighting.

Pore Morphology Analysis

A pore analysis was performed across the full scanned area using a semi-automated edge-detection algorithm. The analysis identified recessed surface features to quantify pore coverage, pore density, radius, void volume, and maximum depth.

Pore detection analysis of the blue climbing grip surface using semi-automated edge detection to identify recessed surface features.

The detected pore locations were mapped across the scanned 5 mm × 5 mm area to evaluate pore coverage, density, and size distribution.

Pore distribution map of the blue climbing grip sample showing detected recessed surface features across a 5 mm by 5 mm scanned area.
Information
Method Circle detection
Features detected Pores, recessed objects
Minimum detection diameter 0.040 mm
Maximum detection diameter 2.000 mm
Number of detected pores 794
Surface coverage 24.208%
Pore density 31.355 particles/mm²
Global Statistics
Parameter Unit Mean Std. Dev. Min Max
Radius mm 0.035 0.035 0.020 0.218
Void volume µm³ 821,872.849 2,495,310.021 11,009.819 2.929 × 10⁷
Maximum depth µm 476.053 305.830 16.132 1044.045

Pores covered 24.208% of the blue grip’s scanned surface, with a pore density of 31.355 particles/mm². The detected pores and cracks were highly heterogeneous in size, volume, and depth, ranging from large crater-like features with a maximum radius of 0.218 mm and void volume greater than 2.9 × 10⁷ µm³ to small pores with a minimum radius of 0.020 mm and void volume of approximately 1.1 × 10⁴ µm³.

This uneven distribution is reflected in the large standard deviation measured for void volume and maximum depth. The pore distribution is bimodal, with one population of fine, deep pores and another population of larger crater-like valleys.

Functional Surface Parameters (Abbott-Firestone curve)

The Abbott-Firestone curve shows the cumulative areal material distribution of the blue climbing grip sample. This analysis defines functional surface parameters including Sk, Spk, and Svk according to ISO 25178-2.

Abbott-Firestone curve for the blue climbing grip sample showing cumulative areal material distribution and functional surface parameters.
Information
Estándar ISO 25178-2
Parameter Value Unit
Sk 522.359 µm
Spk 117.670 µm
Svk 295.209 µm
Smrk1 6.122 %
Smrk2 87.456 %

The chart below shows the peak-valley distribution from the mean plane based on the functional parameters derived from the Abbott-Firestone curve. Valleys are shown in purple, the mean plane in green, and peaks in orange.

Peak-valley distribution map of the blue climbing grip sample showing valleys, mean-plane regions, and peaks derived from Abbott-Firestone functional parameters.
Information
1st threshold Height – c1: 283.646 µm
2nd threshold Height – c2: -238.619 µm
Parameters Unit
Projected area (in %) % 12.544 81.334 6.122
Projected area mm² 3.182 20.629 1.553
Volume of material (in %) % 96.079 48.546 1.514
Volume of material µm³ 1.151 × 10¹⁰ 6.431 × 10⁹ 9.142 × 10⁷

The blue grip sample shows a dominant mean-plane region with fine, deep pores distributed across the surface and localized peak features. Compared with the yellow grip, the blue grip contains a higher projected peak area and a bimodal pore structure, combining fine recessed pores with larger crater-like valleys.

Conclusión

In this application, the NANOVEA JR25 Non-Contact Optical Profiler was used to measure the surface roughness, topography, and pore morphology of yellow and blue bouldering grip samples.

Topographic analysis showed that both grip samples had high surface roughness, with Sa values above 100 µm and Sz values above 1000 µm. Both surfaces also showed an asymmetric height distribution skewed toward valleys, indicating that recessed features played a major role in the measured surface morphology.

The yellow grip sample showed higher pore coverage, with pores covering 47.395% of the scanned surface. Its surface was mainly characterized by average-sized pores distributed across the measured area.

The blue grip sample showed lower pore coverage at 24.208%, but a much higher pore density of 31.355 particles/mm². Its pore distribution was bimodal, with a population of fine, deep pores and a separate population of larger crater-like valleys.

These results show how non-contact 3D optical profilometry can quantify climbing hold surface features that are difficult to evaluate from visual inspection alone, including roughness, pore coverage, pore depth, surface height distribution, and functional topography. The blue grip’s higher porosity and bimodal pore structure make it more likely to absorb moisture and chalk at the contact interface, while its elevated roughness and surface morphology support stable friction for shoe rubber and finger contact. The yellow grip’s lower roughness and flatter profile suggest it is better suited for use as a foothold in slab climbing, where broad surface contact matters more than deep textural engagement.

Frequently Asked Questions About Climbing Hold Surface Roughness

What is climbing hold surface roughness?

Climbing hold surface roughness describes the height variation, texture, pores, asperities, and valleys present on the surface of a climbing grip. These features can influence contact behavior between the hold, shoe rubber, skin, chalk, and moisture.

How can climbing hold surface roughness be measured?

Climbing hold surface roughness can be measured using non-contact 3D optical profilometry. This method reconstructs the surface topography and calculates areal roughness parameters such as Sa, Sz, Sp, Sv, Ssk, and Sku without touching or deforming the sample.

Why use non-contact optical profilometry for climbing hold analysis?

Non-contact optical profilometry is useful for climbing hold analysis because climbing grips can contain deep pores, sharp valleys, rough asperities, and irregular surface texture. A contact stylus may lose contact, fail to reach recessed features, or introduce artifacts on complex surfaces.

What does Sa mean in surface roughness analysis?

Sa is the arithmetic mean height of a surface and is commonly used to describe average areal surface roughness. In this app note, both climbing grip samples showed high Sa values above 100 µm, indicating strongly textured surfaces.

What does Sz mean in optical profilometry results?

Sz is the maximum height of the measured surface, calculated from the highest peak to the deepest valley. In climbing hold surface roughness analysis, Sz helps describe the full vertical range of the grip’s surface texture.

Why is pore morphology important for climbing grips?

Pore morphology can affect how a climbing grip interacts with chalk, sweat, humidity, skin, and shoe rubber. Measuring pore coverage, density, depth, and volume helps quantify surface features that are difficult to evaluate by visual inspection alone.

stent coating adhesion testing failure analysis drug eluting stent coating

Stent Coating Adhesion and Delamination Analysis Using Nano Scratch Testing

Application Note | Stent Coating Adhesion Testing

Stent Coating Adhesion and Delamination Analysis Using Nano Scratch Testing

Quantifying Coating Failure and Adhesion Performance on Drug-Eluting Stents

stent coating adhesion testing nano scratch delamination critical load

Research & Experimental Testing

Doctor Duanjie Li

Visual Design & Editorial

Andrew Shore

Introducción

Blood is carried through arteries from the heart to the rest of the body. Any weakening or blockage of these vessels can pose significant health risks and may become life-threatening. A stent is a small mesh tube inserted into the lumen of a blood vessel to treat narrowed or weakened arteries. Stent implantation is now a widely used procedure to support the arterial wall and restore blood flowᶦ.

Metal stent mesh geometry illustrating the structural complexity of vascular implant design.

Why coating adhesion matters in drug-eluting stents

Drug-eluting stents represent a major advancement in stent technology. They incorporate a biodegradable, biocompatible polymer coating that enables controlled drug release at the arterial site, helping to inhibit intimal thickening and reduce the risk of restenosisᶦᶦ.

A critical concern in these systems is the delamination of the polymer coating from the metallic stent substrate. This coating carries the drug-eluting layer, and its adhesion directly impacts device performance and reliability.

To improve coating adhesion, stents are often designed with complex geometries. In this study, the polymer coating is located at the bottom of grooves within the stent mesh. This configuration presents a significant challenge for adhesion measurement.

A reliable method is required to quantitatively evaluate the interfacial strength between the polymer coating and the metal substrate. The small diameter of the stent mesh, comparable to a human hair, combined with its three-dimensional geometry, requires:

  • ultrafine X-Y positioning accuracy
  • precise control of applied load
  • accurate depth measurement during testing

Measurement Method

Nano scratch testing is performed using the Comprobador mecánico NANOVEA PB1000, in Nano Scratch Mode, to evaluate the cohesive and adhesive strength of the polymer coating on the metal mesh of stent samples.

Controlled scratch measurements are carried out on stent geometries with dimensions comparable to a human hair, enabling precise evaluation of coating adhesion on complex stent structures.

NANOVEA PB1000 Advanced

Comprobador mecánico

Condiciones de prueba

1. Regular Stent Samples

The stent is fixed on the sample stage, with a support wire inserted inside the stent tube to ensure stability during nano scratch testing. The NANOVEA Mechanical Tester is used to perform nano scratch measurements using the parameters summarized in Table 1, to evaluate the cohesive and adhesive strength of the polymer coating on the metal substrate.

ParameterValue
Load typeProgresiva
Initial load0.05 mN
Final load300 and 100 mN
Sliding speed0.5 mm/min
Sliding distance0.5 mm
Indenter geometryCónica
Indenter material (tip)Diamante
Indenter tip radius20 µm
Temperatura24°C (room)

Cuadro 1: Test parameters for nano scratch measurements on regular stent samples

2. Grooved Stent Samples

The SEM image in Fig. 1 shows the cross-section of the stent sample. The stent features a groove with a depth of approximately 30 µm. The polymer coating, with a thickness of 10.8 µm, is located at the bottom of the groove.

Standard 60° conical diamond tips are not sharp enough to reach the bottom of the groove without contacting the sidewalls. Therefore, a sharper 40° conical diamond tip is used in this study (Fig. 2).

Nano scratch measurements are performed using the parameters summarized in Table 2.

Parameter Value
Load type Progresiva
Initial load 0.1 mN
Final load 300 mN
Loading rate 300 mN/min
Scratch length 0.25 mm
Scratch speed 0.25 mm/min
Indenter geometry 40° cone
Indenter material (tip) Diamante
Indenter tip radius 5 µm

Table 2: Test parameters for nano scratch measurements on grooved stent samples

stent groove cross section polymer coating thickness adhesion analysis nano scratch testing

Fig. 1: SEM cross-section of a grooved stent showing polymer coating located at the bottom of the groove, highlighting the challenge of coating adhesion measurement in recessed geometries.

nano scratch diamond tip 40 degree stent groove coating adhesion testing schematic

Fig. 2: Schematic of a 40° conical diamond tip designed for nano scratch testing inside stent grooves, enabling accurate adhesion measurement without sidewall interference.

Resultados y debate

The stent mesh has a diameter of approximately 100 μm, comparable to a human hair. Precise positioning is therefore critical to ensure the scratch test is performed at the center of the stent mesh. The NANOVEA Mechanical Tester provides X–Y positioning accuracy down to 0.25 μm, enabling accurate test placement under the integrated optical microscope.

1. Regular Stent Samples

Nano scratch testing is performed with a progressively increasing load up to 300 mN. The full scratch track on the stent is shown in Fig. 3a, while failure behavior at different stages is presented in Fig. 3b and 3c.

Two critical loads are identified:

  • Lc1: the load at which the first visible damage appears on the coating
  • Lc2: the load at which the coating is fully removed and the substrate is exposed

The evolution of coefficient of friction (COF) and penetration depth is shown in Fig. 4, providing insight into the progression of coating failure during the test.

The first signs of coating damage appear at Lc1 ≈ 14.5 mN. As the applied load increases, the diamond tip progressively penetrates the polymer coating, resulting in a wider and deeper scratch track. During this phase, the COF increases from approximately 0.05 to 0.7.

At Lc2 ≈ 78.1 mN, the coating is fully delaminated from the metal substrate. Beyond this point, as the load continues to increase, both COF and penetration depth remain relatively stable due to the mechanical support of the underlying metal substrate.

nano scratch track stent coating progressive load adhesion testing

(a) Full Scratch Track

(b) Lc1 ≈ 14.5 mN

stent coating delamination lc2 nano scratch 78.1 mN adhesion testing

(c) Lc2 ≈ 78.1 mN

Fig. 3: Nano scratch track on a stent coating under progressively increasing load, showing (a) full scratch path, (b) initial coating failure at Lc1 ≈ 14.5 mN, and (c) complete coating delamination at Lc2 ≈ 78.1 mN.

nano scratch testing stent coating coefficient of friction depth progression adhesion failure

Fig. 4: Evolution of coefficient of friction (COF) and penetration depth during nano scratch testing of a stent coating under progressively increasing load, showing the progression of coating failure and transition to substrate support.

Failures during nano scratch testing up to a maximum load of 300 mN occur at critical loads below 100 mN. To enable a more quantitative comparison of coating performance, additional tests are performed with a maximum load of 100 mN on two stent samples, referred to as Sample 1 and Sample 2.

Fig. 5 compares the scratch tracks of Sample 1 and Sample 2 after nano scratch testing. Sample 1 exhibits the first sign of coating damage at a critical load of Lc1 ≈ 13.2 mN, while Sample 2 shows initial failure at a higher load of Lc1 ≈ 21.1 mN.

Coating delamination occurs at 62.5 mN for Sample 1. In contrast, the coating on Sample 2 remains intact throughout the test, continuing to protect the metal substrate under the same loading conditions.

This behavior is further reflected in the evolution of coefficient of friction (COF) and penetration depth, as shown in Fig. 6. When the diamond tip penetrates through the coating and contacts the metal substrate in Sample 1, the COF reaches a peak while the penetration depth decreases due to the increased stiffness of the underlying substrate.

stent coating sample 1 early failure nano scratch track delamination adhesion testing

(a) Sample 1 – Early Coating Failure

stent coating sample 2 high adhesion nano scratch track minimal damage testing

(b) Sample 2 – Improved Coating Integrity

Fig. 5: Comparison of nano scratch tracks for two stent coatings, showing (a) early coating failure and delamination in Sample 1, and (b) improved coating integrity in Sample 2 under the same loading conditions.

nano scratch testing stent coating COF depth comparison sample 1 sample 2 adhesion performance

Fig. 6: Comparison of coefficient of friction (COF) and penetration depth for Sample 1 and Sample 2 during nano scratch testing, showing earlier substrate contact and higher friction response in Sample 1, indicating weaker coating adhesion.

2. Grooved Stent Samples

As shown in Fig. 1 and Fig. 7, the grooved stent mesh has a diameter of approximately 90 μm, comparable to a human hair. The groove has a width of ~50 μm and a depth of 30 μm. This geometry presents a significant challenge for nano scratch testing, particularly for evaluating coating adhesion at the bottom of the groove.

Precise positioning is critical to locate the scratch test within the groove. The nano scratch test is performed with a progressively increasing load up to 300 mN. The full scratch tracks of grooved stent Samples 3 and 4 are compared in Fig. 7.

The critical load Lc is defined as the load at which the coating fails and the substrate becomes exposed. The evolution of normal load and penetration depth, shown in Fig. 8, provides further insight into the progression of coating failure during testing.

As the applied load increases, the diamond tip progressively penetrates the polymer coating, resulting in a deeper scratch track. When the critical load Lc is reached, the coating delaminates from the metal substrate.

Sample 3 exhibits coating failure at Lc ≈ 126 mN, while Sample 4 fails at a higher load of Lc ≈ 173 mN. This difference indicates stronger adhesion of the coating in Sample 4.

The measured critical loads enable quantitative comparison of coating adhesion performance. Under the same testing conditions, the coating on Sample 4 demonstrates higher resistance to delamination, making it the better-performing candidate in this study.

stent groove coating failure sample 3 nano scratch 126 mN adhesion testing

(c) Sample 3 – Coating Failure in Groove (Lc ≈ 126 mN)

stent groove coating adhesion sample 4 nano scratch 173 mN minimal failure testing

(d) Sample 4 – Higher Adhesion in Groove (Lc ≈ 173 mN)

Fig. 7: Nano scratch tracks inside stent grooves for Samples 3 and 4, showing (c) coating failure at Lc ≈ 126 mN in Sample 3 and (d) higher adhesion with delayed failure at Lc ≈ 173 mN in Sample 4.

(a) Sample 3 – Earlier Coating Failure (Lc ≈ 126 mN)

(b) Sample 4 – Delayed Failure and Higher Adhesion (Lc ≈ 173 mN)

Fig. 8: Evolution of normal load and penetration depth during nano scratch testing inside stent grooves for Samples 3 and 4, showing earlier coating failure in Sample 3 and delayed failure at higher load in Sample 4. The vertical green line indicates the critical load (Lc) where coating delamination occurs.

Conclusión

This study demonstrates the ability of the NANOVEA Mechanical Tester to quantitatively evaluate the cohesive and adhesive strength of polymer coatings on both regular and grooved stent geometries using nano scratch testing.

The recessed geometry of the stent grooves, approximately 50 μm wide and 30 μm deep, presents a significant challenge for coating adhesion measurement. The high X–Y positioning accuracy of 0.25 μm enables precise placement of the scratch test within these confined regions, allowing direct evaluation of coating performance where failure is most critical.

By applying a controlled, progressively increasing load, critical loads associated with coating failure can be identified and compared across samples. This approach enables reliable differentiation of coating adhesion performance and interfacial integrity, even on small, complex stent structures.

Referencias

[I] http://www.nhlbi.nih.gov/health/health-topics/topics/stents
[II] http://www.scielo.org.mx/scielo.php?script=sci_arttext&pid=S1405-99402006000300008

Frequently Asked Questions About Stent Coating Adhesion Testing

What is stent coating adhesion testing?

Stent coating adhesion testing evaluates how strongly a polymer coating is bonded to the metal substrate of a stent. Techniques such as nano scratch testing quantify the load at which coating damage and delamination occur, providing measurable indicators of adhesion strength.

What is critical load (Lc) in nano scratch testing?

Critical load (Lc) is the applied load at which a coating fails during a scratch test.

  • Lc1 corresponds to the first visible damage in the coating
  • Lc2 indicates complete coating removal and exposure of the substrate

These values are used to quantify and compare coating adhesion performance.

Why is coating adhesion important in drug-eluting stents?

Coating adhesion directly affects the reliability of drug-eluting stents. Poor adhesion can lead to coating delamination, which may compromise controlled drug release and increase the risk of device failure.

How do you measure coating adhesion inside stent grooves?

Measuring adhesion inside stent grooves requires high positioning accuracy and appropriate indenter geometry. Nano scratch testing with sharp diamond tips allows access to recessed coating regions, enabling direct evaluation of adhesion within complex stent geometries.

What does coefficient of friction (COF) indicate in scratch testing?

The coefficient of friction (COF) reflects changes in surface interaction during the scratch test. A sudden increase in COF often indicates coating failure and contact between the indenter and the underlying metal substrate.

How can nano scratch testing compare different coating formulations?

Nano scratch testing enables direct comparison of coatings by measuring critical loads under controlled conditions. Higher critical loads indicate stronger adhesion and improved resistance to delamination, allowing selection of better-performing coating systems.

Dentist holding dental model for tooth surface roughness analysis and 3D reconstruction

Dental Surface Roughness Measurement & 3D Tooth Topography

Application Note | Dental Surface Characterization

Dental Surface Roughness Measurement and Full 3D Tooth Topography

Surface Roughness Analysis Using Non-Contact Optical Profilometry

Dental surface roughness measurement and 3D molar reconstruction using optical profilometry

Preparado por

Walter Alabiso, PhD; Davide Morrone, MPhys; Andrew Shore, MA

Introducción

The ability to accurately characterize tooth surfaces, including micro-roughness and 3D surface topography at the nanometer scale, enables advanced research and applications in orthodontics and dental materials science. Non-contact optical profilometry provides a precise method for measuring dental surface roughness and analyzing tooth surface morphology without damaging delicate structures. These measurements support the development of composite dental materials that replicate the natural surface roughness of enamel, as well as the design and fabrication of patient-specific dental casts and restorative components.

Low surface roughness plays a primary role in limiting bacterial adhesion and plaque formation, thereby reducing the risk of cavities. An increase in average roughness (Ra) above 2 µm leads to a steep increase in biofilm formation in vivo.¹ An Ra of 0.2 µm is considered the threshold value below which no further reduction in bacterial adhesion can be expected.²

Reconstruction of the tooth’s 3D surface topography enables the fabrication of dental casts, which are essential for accurate diagnosis, treatment planning, and the fabrication of dental appliances.

Non-Contact Optical Profilometry for Dental Surface Analysis

The present study illustrates the potential of NANOVEA’s high-precision non-contact optical profilometers for dental surface roughness measurement and 3D tooth topography analysis. Chromatic Light technology offers significant advantages over classical touch probe techniques. It acquires data points from deep crevices and complex geometries without introducing measurement errors or artifacts caused by local plastic deformation and without requiring extensive data manipulation.

Compared to focus variation systems, single-point optical sensing provides superior lateral and height accuracy, with X/Y resolution below 0.5 µm, maximum vertical resolution of 1.9 nm, and the ability to measure surface angles up to 87°. The technique is effective on transparent, opaque, specular, diffusive, polished, and rough dental surfaces, making it well suited for comprehensive dental surface characterization.

Measurement Method

En esta aplicación, el NANOVEA JR25 Non-Contact Optical Profiler was used to analyze the surface roughness and 3D surface topography of an adult human molar previously affected by tooth decay. The side of the tooth was scanned using a PS2–MG140 single-point optical sensor to measure surface roughness parameters over a defined region of interest and along multiple line profiles.

The crown of the tooth was then scanned and reconstructed using a PS5–MG35 single-point optical sensor, which is suited for larger-area acquisition and full 3D tooth topography measurement.


NANOVEA JR25 Portable
Perfilómetro óptico

Surface Measurement Using NANOVEA Optical Profilometer

Surface roughness measurements were performed on the lateral side of the molar crown, followed by full 3D reconstruction of the crown surface. Separate single-point optical sensors were used to optimize measurement accuracy for both localized roughness analysis and large-area surface topography acquisition.

PS2 – MG140

Surface roughness analysis by area and parallel line profiles on the side of the tooth’s crown.

PS5 – MG35

Full 3D surface reconstruction of the tooth’s crown.

Parámetros de medición

The following measurement parameters were used for localized surface roughness analysis and full 3D surface reconstruction of the molar crown using NANOVEA single-point optical sensors.

ParameterRoughness Analysis (Area)Roughness Analysis (Profiles)Full 3D Reconstruction
Optical PenPS2-MG140PS2-MG140PS5-MG35
Z-Range [µm]30030010000
X-Distance [mm]2.003.007.50
X-Step Size [µm]1.701.7010.00
Y-Distance [mm]2.001.007.00
Y-Step Size [µm]1.70100.0010.00
Averaging (Avg)111
Measurement TypeDirectDirectDirect
Acquisition ModeSingle FrequencySingle FrequencyDual Frequency
Acquisition Rate [Hz]200200100–400
Light Intensity [%]100100100

Optical Profilometry Results

Surface Roughness Analysis (AREA)

 The single-point optical sensor PS2 was used to investigate fine features of the tooth’s side surface. The following picture represents a false-color 2D map of the scanned region:

False-color 2D height map of scanned tooth surface region

A least-squares degree-8 polynomial form removal was applied to isolate the surface roughness component. The roughness filters S-Gaussian 2.5 µm and L-Gaussian 0.8 mm were then applied according to ISO 25178. The resulting filtered surface and corresponding roughness parameters are presented below.

ISO 25178 – Roughness (S-L)
S-filter (λs): Gaussian, 2.5 µm
F: [Workflow] Form removed (LS-poly 8)
L-filter (λc): Gaussian, 0.8 mm
Height Parameters
Sq2.433µmAltura media cuadrática
Ssk-0.102 Skewness
Código3.715 Kurtosis
Sp18.861µmAltura máxima del pico
Sv16.553µmMaximum pit depth
Sz35.414µmAltura máxima
Sa1.888µmAltura media aritmética

The average surface roughness Sa is 1.888 µm, while the peak-to-valley height Sz reaches 35.414 µm.

A 3D surface rendering of the filtered area is shown below for visualization.

3D rendering of ISO 25178 filtered tooth surface roughness

Roughness Analysis (Profiles)

Surface roughness profiles were measured using a series of 11 parallel line scans along the X direction on the side of the tooth. The false-color 2D surface map of the raw scan is shown below.

False-color 2D raw scan of tooth surface for line roughness profiles

The surface form was removed using a least-squares 8-degree polynomial prior to applying the metrological filters, leaving the residual surface shown below.

A statistical analysis of the measured surface roughness profiles reveals the following line roughness parameters.

Overlay of multiple tooth surface roughness profiles for statistical analysis

ISO 4287 – Roughness (S-L)
F: Ninguno
S-filter (λs): Gaussian, 2.5 µm
L-filter (λc): Gaussian, 0.8 mm
Evaluation length: All λc (3)
Amplitude Parameters – Roughness Profile
  DescriptionMeanStd devMinMax
RpµmMaximum peak height of the roughness profile5.6830.7614.3156.610
RvµmMaximum valley depth of the roughness profile6.2421.0094.7018.438
RzµmMaximum height of roughness profile11.9251.6769.12315.048
RaµmArithmetic mean deviation of the roughness profile2.0630.2971.7102.629
RqµmRoot-mean-square (RMS) deviation of the roughness profile2.5230.3612.0573.175

ISO 4287 – Roughness (S-L)
F: Ninguno
S-filter (λs): Gaussian, 2.5 µm
L-filter (λc): Gaussian, 0.8 mm
Evaluation length: All λc (3)
Amplitude Parameters – Roughness Profile
Rpµm
Maximum peak height of the roughness profile
Mean5.683
Std dev0.761
Min4.315
Max6.610
Rvµm
Maximum valley depth of the roughness profile
Mean6.242
Std dev1.009
Min4.701
Max8.438
Rzµm
Maximum height of roughness profile
Mean11.925
Std dev1.676
Min9.123
Max15.048
Raµm
Arithmetic mean deviation of the roughness profile
Mean2.063
Std dev0.297
Min1.710
Max2.629
Rqµm
Root-mean-square (RMS) deviation of the roughness profile
Mean2.523
Std dev0.361
Min2.057
Max3.175

The value of Ra is consistent with the Sa value extracted from the surface area measurement.

Different metrological filters can be applied to distinguish between macroscopic waviness and microscopic surface roughness. For example, a coarser filter cut-off, such as the 8 mm cut-off used with the Robust Gaussian order-2 filter, produces a smoother waviness profile (red) that is less sensitive to sharp local variations and follows the original surface profile more loosely.

Comparison of waviness and roughness profiles on tooth surface using coarse filter

Alternatively, a finer cut-off (e.g., 0.08 mm) enables the analysis of micro-roughness by removing the waviness component that follows the original profile at a larger scale, leaving the finer surface roughness features of the tooth visible.

The microroughness analysis obtained using a 0.08 mm L-Gaussian filter is presented below.

Final microroughness profile of tooth surface after filtering

ISO 4287 – Roughness (S-L)
F: Ninguno
S-filter (λs): Gaussian, 2.5 µm
L-filter (λc): Gaussian, 0.08 mm
Evaluation length: All λc (37)
Amplitude Parameters – Roughness Profile
  DescriptionMeanStd devMinMax
RpµmMaximum peak height of the roughness profile1.5820.1221.3421.748
RvµmMaximum valley depth of the roughness profile1.4660.1191.2541.661
RzµmMaximum height of roughness profile3.0490.1962.8203.409
RaµmArithmetic mean deviation of the roughness profile0.4950.0470.4230.597
RqµmRoot-mean-square (RMS) deviation of the roughness profile0.6430.0560.5620.762

ISO 4287 – Roughness (S-L)
F: Ninguno
S-filter (λs): Gaussian, 2.5 µm
L-filter (λc): Gaussian, 0.8 mm
Evaluation length: All λc (3)
Amplitude Parameters – Roughness Profile
Rpµm
Maximum peak height of the roughness profile
Mean5.683
Std dev0.761
Min4.315
Max6.610
Rvµm
Maximum valley depth of the roughness profile
Mean6.242
Std dev1.009
Min4.701
Max8.438
Rzµm
Maximum height of roughness profile
Mean11.925
Std dev1.676
Min9.123
Max15.048
Raµm
Arithmetic mean deviation of the roughness profile
Mean2.063
Std dev0.297
Min1.710
Max2.629
Rqµm
Root-mean-square (RMS) deviation of the roughness profile
Mean2.523
Std dev0.361
Min2.057
Max3.175

Full 3D Tooth Surface Topography Reconstruction

The extended Z-scan range of the PS5 optical sensor enables high-fidelity scanning of the entire tooth crown surface. The resulting 3D surface topography is shown below.

False-color surface topography map of full tooth crown measured with optical profilometer

2D VIEW: 2D surface map of the tooth crown measured with optical profilometry

3D surface reconstruction of molar crown from optical profilometer scan

3D VIEW: High-fidelity 3D rendering of the molar crown surface obtained with optical profilometry

Conclusión

In this application, the NANOVEA JR25 Non-Contact Optical Profiler was used to measure the surface roughness and 3D surface topography of an adult human molar.

Both the area scan and the line profile analysis revealed a roughness Rq of approximately 2.5 µm and an Ra of about 1.9–2.0 µm. These values are consistent with results reported in the literature.³ The use of a narrower L-Gaussian filter with an 80 µm cut-off enabled further investigation of micro-roughness, revealing an Rq of 0.643 µm and an Ra of 0.495 µm.

The full 3D surface topography of the molar crown was reconstructed with high fidelity. The high measurement resolution allows detection of fine surface features and crevices. The resulting surface data can be easily processed and exported as STL files, enabling the design and fabrication of customized dental devices and restorative components.

Referencias

[1] Shin, B.W., et al. Surface Roughness of Prefabricated Pediatric Zirconia Crowns Following Simulated Toothbrushing. Pediatric Dentistry 44.5 (2022): 363–367.
[2] Bollen, C.M.L., Paul Lambrechts, and Marc Quirynen. Comparison of surface roughness of oral hard materials to the threshold surface roughness for bacterial plaque retention: A review of the literature. Dental Materials 13.4 (1997): 258–269.
[3] Suputtamongkol, K., et al. Surface roughness resulting from wear of lithia-disilicate-based posterior crowns. Wear 269.3–4 (2010): 317–322.

Frequently Asked Questions About Dental Surface Roughness Measurement

What is dental surface roughness measurement?

Dental surface roughness measurement quantifies the microscopic texture of tooth surfaces using parameters such as Ra, Rq, and Sa. Optical profilometers measure these features without contacting the surface, allowing accurate analysis of enamel, restorative materials, and dental crowns.

Why use optical profilometry to measure tooth roughness?

Optical profilometry provides non-contact surface measurement with nanometer-scale vertical resolution. It captures 2D surface maps and full 3D surface topography of dental structures without damaging soft or polished surfaces.

What roughness parameters are used for dental surface analysis?

Common roughness parameters include Ra (arithmetic mean roughness), Rq (root mean square roughness), Sa (areal roughness), and Sz (maximum surface height). These parameters help evaluate enamel wear, plaque adhesion risk, and the performance of restorative materials.

Why is surface roughness important in dentistry?

Surface roughness affects plaque retention, wear resistance, and the long-term performance of dental restorations. Controlling micro-roughness can reduce bacterial adhesion and improve the durability of dental materials.

Need Reliable Surface Roughness Measurement for Dental Materials?

Análisis de superficies granalladas

ANÁLISIS DE SUPERFICIES GRANALLADAS

UTILIZANDO UN PERFILÓMETRO 3D SIN CONTACTO

Preparado por

CRAIG LEISING

INTRODUCCIÓN

El shot peening es un proceso en el que un sustrato se bombardea con perlas esféricas de metal, vidrio o cerámica -comúnmente denominadas "granalla"- a una fuerza destinada a inducir plasticidad en la superficie. El análisis de las características antes y después del granallado proporciona información crucial para mejorar la comprensión y el control del proceso. La rugosidad de la superficie y el área de cobertura de los hoyuelos dejados por la granalla son aspectos de especial interés.

Importancia del perfilómetro 3D sin contacto para el análisis de superficies de granallado

A diferencia de los perfilómetros de contacto tradicionales, que se han utilizado tradicionalmente para el análisis de superficies granalladas, la medición 3D sin contacto proporciona una imagen 3D completa para ofrecer una comprensión más exhaustiva del área de cobertura y la topografía de la superficie. Sin capacidades 3D, una inspección se basará únicamente en información 2D, que es insuficiente para caracterizar una superficie. Comprender la topografía, el área de cobertura y la rugosidad en 3D es el mejor enfoque para controlar o mejorar el proceso de peening. NANOVEA Perfilómetros 3D sin contacto utilizan la tecnología de luz cromática con una capacidad única para medir ángulos pronunciados que se encuentran en superficies mecanizadas y granalladas. Además, cuando otras técnicas no proporcionan datos fiables debido al contacto de la sonda, la variación de la superficie, el ángulo o la reflectividad, los perfilómetros NANOVEA lo consiguen.

OBJETIVO DE MEDICIÓN

En esta aplicación, el perfilómetro sin contacto NANOVEA ST400 se utiliza para medir el material en bruto y dos superficies granalladas de forma diferente para una revisión comparativa. Hay una lista interminable de parámetros de superficie que se pueden calcular automáticamente después de la exploración de la superficie 3D. Aquí, revisaremos la superficie 3D y seleccionaremos las áreas de interés para su posterior análisis, incluyendo la cuantificación e investigación de la rugosidad, los hoyuelos y el área superficial.

NANOVEA ST400 Estándar
Perfilómetro óptico 3D

LA MUESTRA

Ensayos de superficies granalladas

RESULTADOS

SUPERFICIE DE ACERO

Rugosidad superficial granallada
Caracterización de superficies granalladas

ISO 25178 PARÁMETROS DE ROUGNESS 3D

SA 0,399 μm Rugosidad media
Sq 0,516 μm Rugosidad RMS
Sz 5,686 μm Máximo de pico a valle
Sp 2,976 μm Altura máxima del pico
Sv 2,711 μm Profundidad máxima de la fosa
Código 3.9344 Kurtosis
Ssk -0.0113 Skewness
Sal 0,0028 mm Longitud de autocorrelación
Str 0.0613 Relación de aspecto de la textura
Sdar 26,539 mm² Superficie
Svk 0,589 μm Reducción de la profundidad del valle
 

RESULTADOS

SUPERFICIE GRANALLADA 1

Perfil de superficie granallada
Perfilometría de superficies granalladas

COBERTURA SUPERFICIAL 98.105%

Estudio de superficies granalladas

ISO 25178 PARÁMETROS DE ROUGNESS 3D

Sa 4,102 μm Rugosidad media
Sq 5,153 μm Rugosidad RMS
Sz 44,975 μm Máximo de pico a valle
Sp 24,332 μm Altura máxima del pico
Sv 20,644 μm Profundidad máxima de la fosa
Código 3.0187 Kurtosis
Ssk 0.0625 Skewness
Sal 0,0976 mm Longitud de autocorrelación
Str 0.9278 Relación de aspecto de la textura
Sdar 29,451 mm² Superficie
Svk 5,008 μm Reducción de la profundidad del valle

RESULTADOS

SUPERFICIE GRANALLADA 2

Ensayo de superficie granallada
Análisis de superficies granalladas

COBERTURA SUPERFICIAL 97.366%

Metrología de superficies granalladas

ISO 25178 PARÁMETROS DE ROUGNESS 3D

Sa 4,330 μm Rugosidad media
Sq 5,455 μm Rugosidad RMS
Sz 54,013 μm Máximo de pico a valle
Sp 25,908 μm Altura máxima del pico
Sv 28,105 μm Profundidad máxima de la fosa
Código 3.0642 Kurtosis
Ssk 0.1108 Skewness
Sal 0,1034 mm Longitud de autocorrelación
Str 0.9733 Relación de aspecto de la textura
Sdar 29,623 mm² Superficie
Svk 5,167 μm Reducción de la profundidad del valle

CONCLUSIÓN

En esta aplicación de análisis de superficies granalladas, hemos demostrado cómo el perfilómetro 3D sin contacto NANOVEA ST400 caracteriza con precisión tanto la topografía como los detalles nanométricos de una superficie granallada. Es evidente que tanto la superficie 1 como la superficie 2 tienen un impacto significativo en todos los parámetros reportados aquí en comparación con el material en bruto. Un simple examen visual de las imágenes revela las diferencias entre las superficies. Esto se confirma observando el área de cobertura y los parámetros enumerados. En comparación con la superficie 2, la superficie 1 presenta una rugosidad media inferior (Sa), abolladuras menos profundas (Sv) y un área de superficie reducida (Sdar), pero un área de cobertura ligeramente superior.

A partir de estas mediciones de superficie en 3D, las áreas de interés pueden identificarse fácilmente y someterse a una amplia gama de mediciones, como Rugosidad, Acabado, Textura, Forma, Topografía, Planitud, Alabeo, Planaridad, Volumen, Paso-Altura y otras. Se puede elegir rápidamente una sección transversal 2D para realizar un análisis detallado. Esta información permite una investigación exhaustiva de las superficies granalladas, utilizando una gama completa de recursos de medición de superficies. Las áreas específicas de interés pueden examinarse más a fondo con un módulo AFM integrado. Los perfilómetros NANOVEA 3D ofrecen velocidades de hasta 200 mm/s. Se pueden personalizar en términos de tamaño, velocidades, capacidades de escaneado e incluso pueden cumplir las normas de Sala Limpia de Clase 1. También están disponibles opciones como el transportador de indexación y la integración para uso en línea o en línea.

Un agradecimiento especial al Sr. Hayden de IMF por suministrar la muestra que aparece en esta nota. Industrial Metal Finishing Inc. | indmetfin.com

Morfología de la superficie de la pintura

MORFOLOGÍA DE LA SUPERFICIE DE LA PINTURA

SEGUIMIENTO AUTOMATIZADO DE LA EVOLUCIÓN EN TIEMPO REAL
USO DEL PERFILÓMETRO NANOVEA 3D

Morfología de la superficie de la pintura

Preparado por

DUANJIE LI, Doctor

INTRODUCCIÓN

Las propiedades protectoras y decorativas de la pintura desempeñan un papel importante en diversos sectores, como el de la automoción, el naval, el militar y el de la construcción. Para conseguir las propiedades deseadas, como resistencia a la corrosión, protección UV y resistencia a la abrasión, las fórmulas y arquitecturas de la pintura se analizan, modifican y optimizan cuidadosamente.

IMPORTANCIA DEL PERFILÓMETRO 3D SIN CONTACTO PARA EL ANÁLISIS DE LA MORFOLOGÍA SUPERFICIAL DE LA PINTURA DE SECADO

La pintura suele aplicarse en forma líquida y se somete a un proceso de secado, que implica la evaporación de disolventes y la transformación de la pintura líquida en una película sólida. Durante el proceso de secado, la superficie de la pintura cambia progresivamente de forma y textura. Se pueden conseguir diferentes acabados y texturas superficiales utilizando aditivos para modificar la tensión superficial y las propiedades de fluidez de la pintura. Sin embargo, en los casos de una receta de pintura mal formulada o un tratamiento superficial inadecuado, pueden producirse fallos no deseados en la superficie de la pintura.

La monitorización precisa in situ de la morfología de la superficie de la pintura durante el periodo de secado puede proporcionar información directa sobre el mecanismo de secado. Además, la evolución en tiempo real de las morfologías superficiales es una información muy útil en diversas aplicaciones, como la impresión 3D. El sistema NANOVEA Perfilómetros 3D sin contacto medir la morfología de la superficie pictórica de los materiales sin tocar la muestra, evitando cualquier alteración de la forma que puedan provocar las tecnologías de contacto, como un palpador deslizante.

OBJETIVO DE MEDICIÓN

En esta aplicación, el perfilómetro sin contacto NANOVEA ST500, equipado con un sensor óptico de línea de alta velocidad, se utiliza para monitorizar la morfología de la superficie de la pintura durante su periodo de secado de 1 hora. Mostramos la capacidad del perfilómetro sin contacto NANOVEA para proporcionar mediciones automatizadas de perfiles 3D en tiempo real de materiales con cambio continuo de forma.

NANOVEA ST500 Gran superficie
Perfilómetro óptico 3D

RESULTADOS Y DEBATE

La pintura se aplicó sobre la superficie de una chapa metálica, seguida inmediatamente de mediciones automatizadas de la evolución de la morfología de la pintura en secado in situ utilizando el perfilómetro sin contacto NANOVEA ST500 equipado con un sensor de línea de alta velocidad. Se había programado una macro para medir y registrar automáticamente la morfología 3D de la superficie a intervalos de tiempo específicos: 0, 5, 10, 20, 30, 40, 50 y 60 min. Este procedimiento de escaneado automatizado permite a los usuarios realizar tareas de escaneado automáticamente ejecutando procedimientos establecidos en secuencia, lo que reduce significativamente el esfuerzo, el tiempo y los posibles errores del usuario en comparación con las pruebas manuales o los escaneados repetidos. Esta automatización resulta extremadamente útil para mediciones a largo plazo que implican múltiples exploraciones a diferentes intervalos de tiempo.

El sensor óptico de línea genera una línea brillante formada por 192 puntos, como se muestra en la FIGURA 1. Estos 192 puntos luminosos escanean simultáneamente la superficie de la muestra, lo que aumenta significativamente la velocidad de escaneado. Esto garantiza que cada escaneado 3D se complete rápidamente para evitar cambios sustanciales en la superficie durante cada escaneado individual.

Análisis del revestimiento de pintura con un perfilómetro 3D

FIGURA 1: Sensor óptico de líneas que escanea la superficie de la pintura en secado.

La vista en falso color, la vista en 3D y el perfil en 2D de la topografía de la pintura secándose en momentos representativos se muestran en la FIGURA 2, FIGURA 3 y FIGURA 4, respectivamente. El falso color en las imágenes facilita la detección de características que no son fácilmente discernibles. Los diferentes colores representan variaciones de altura en diferentes áreas de la superficie de la muestra. La vista 3D proporciona una herramienta ideal para que los usuarios observen la superficie de la pintura desde diferentes ángulos. Durante los primeros 30 minutos de la prueba, los falsos colores de la superficie de la pintura cambian gradualmente de tonos más cálidos a tonos más fríos, lo que indica una disminución progresiva de la altura con el paso del tiempo en este periodo. Este proceso se ralentiza, como demuestra el leve cambio de color al comparar la pintura a los 30 y 60 minutos.

Los valores de la altura media de la muestra y de la rugosidad Sa en función del tiempo de secado de la pintura se representan en la FIGURA 5. El análisis completo de la rugosidad de la pintura después de 0, 30 y 60 min de tiempo de secado se enumeran en la TABLA 1. Puede observarse que la altura media de la superficie de la pintura disminuye rápidamente de 471 a 329 µm en los primeros 30 min de tiempo de secado. La textura de la superficie se desarrolla al mismo tiempo que se vaporiza el disolvente, lo que provoca un aumento del valor Sa de la rugosidad de 7,19 a 22,6 µm. El proceso de secado de la pintura se ralentiza a partir de entonces, lo que provoca una disminución gradual de la altura de la muestra y del valor Sa hasta 317 µm y 19,6 µm, respectivamente, a los 60 min.

Este estudio pone de relieve las capacidades del perfilómetro 3D sin contacto NANOVEA para monitorizar en tiempo real los cambios de la superficie 3D de la pintura en proceso de secado, proporcionando información valiosa sobre el proceso de secado de la pintura. Al medir la morfología de la superficie sin tocar la muestra, el perfilómetro evita introducir alteraciones de forma en la pintura sin secar, lo que puede ocurrir con tecnologías de contacto como el palpador deslizante. Este enfoque sin contacto garantiza un análisis preciso y fiable de la morfología de la superficie de la pintura en proceso de secado.

Morfología de la superficie de la pintura
Morfología del revestimiento de pintura

FIGURA 2: Evolución de la morfología de la superficie de la pintura en secado a diferentes tiempos.

Caracterización de la superficie de la pintura
Perfil de la superficie de pintura
Análisis de la superficie de la pintura

FIGURA 3: Vista en 3D de la evolución de la superficie de la pintura a diferentes tiempos de secado.

Perfilometría de superficies de pintura

FIGURA 4: Perfil 2D de la muestra de pintura tras diferentes tiempos de secado.

Estudio de la superficie de la pintura

FIGURA 5: Evolución de la altura media de la muestra y del valor de rugosidad Sa en función del tiempo de secado de la pintura.

ISO 25178 - Parámetros de textura superficial

Tiempo de secado (min) 0 5 10 20 30 40 50 60
Sq (µm) 7.91 9.4 10.8 20.9 22.6 20.6 19.9 19.6
Código 26.3 19.8 14.6 11.9 10.5 9.87 9.83 9.82
Sp (µm) 97.4 105 108 116 125 118 114 112
Sv (µm) 127 70.2 116 164 168 138 130 128
Sz (µm) 224 175 224 280 294 256 244 241
Sa (µm) 4.4 5.44 6.42 12.2 13.3 12.2 11.9 11.8

Sq - Altura media cuadrática | Sku - Kurtosis | Sp - Altura máxima del pico | Sv - Altura máxima del foso | Sz - Altura máxima | Sv - Altura media aritmética

TABLA 1: Rugosidad de la pintura a diferentes tiempos de secado.

CONCLUSIÓN

En esta aplicación, hemos mostrado las capacidades del perfilómetro 3D sin contacto NANOVEA ST500 para supervisar la evolución de la morfología de la superficie de la pintura durante el proceso de secado. El sensor óptico de línea de alta velocidad, que genera una línea con 192 puntos de luz que escanean la superficie de la muestra simultáneamente, ha hecho que el estudio sea eficiente en cuanto al tiempo, al tiempo que garantiza una precisión inigualable.

La función macro del software de adquisición permite programar mediciones automatizadas de la morfología de la superficie 3D in situ, por lo que resulta especialmente útil para mediciones a largo plazo que impliquen múltiples exploraciones a intervalos de tiempo específicos. Reduce significativamente el tiempo, el esfuerzo y los posibles errores del usuario. Los cambios progresivos en la morfología de la superficie se supervisan continuamente y se registran en tiempo real a medida que se seca la pintura, lo que proporciona información valiosa sobre el mecanismo de secado de la pintura.

Los datos mostrados aquí representan sólo una fracción de los cálculos disponibles en el software de análisis. Los perfilómetros NANOVEA son capaces de medir prácticamente cualquier superficie, ya sea transparente, oscura, reflectante u opaca.

Cartografía de desgaste progresivo de pavimentos mediante tribómetro

Pruebas de desgaste de suelos

Cartografía de desgaste progresivo de suelos mediante tribómetro con perfilómetro integrado

pruebas de desgaste de suelos

Preparado por

FRANK LIU

INTRODUCCIÓN

Los materiales de los suelos están diseñados para ser duraderos, pero a menudo sufren el desgaste de actividades cotidianas como el movimiento y el uso de muebles. Para garantizar su longevidad, la mayoría de los tipos de suelos tienen una capa protectora que resiste los daños. Sin embargo, el grosor y la durabilidad de la capa de desgaste varían en función del tipo de flooring y del nivel de traffic de los pies. Además, las distintas capas de la estructura del revestimiento, como los revestimientos UV, las capas decorativas y el esmalte, tienen diferentes índices de desgaste. Ahí es donde entra en juego el mapeo progresivo del desgaste. Utilizando el tribómetro NANOVEA T2000 con un Profilómetro 3D sin contactoGracias a la investigación, es posible realizar un seguimiento preciso y un análisis del rendimiento y la longevidad de los materiales de los sistemas de agarre. Al proporcionar información detallada sobre el comportamiento ante el desgaste de los distintos materiales de los sistemas de agarre, los científicos y los profesionales técnicos pueden tomar decisiones más fundamentadas a la hora de seleccionar y diseñar nuevos sistemas de agarre.

IMPORTANCIA DE LA CARTOGRAFÍA DEL DESGASTE PROGRESIVO DE LOS PANELES DE SUELO

Los ensayos de suelos se han centrado tradicionalmente en la tasa de desgaste de una muestra para determinar su durabilidad frente al desgaste. Sin embargo, el mapeo progresivo del desgaste permite analizar la tasa de desgaste de la muestra a lo largo de la prueba, lo que proporciona información valiosa sobre su comportamiento frente al desgaste. Este análisis en profundidad permite establecer correlaciones entre los datos de fricción y la tasa de desgaste, lo que puede identificar las causas fundamentales del desgaste. Cabe señalar que las tasas de desgaste no son constantes a lo largo de las pruebas de desgaste. Por lo tanto, la observación de la progresión del desgaste proporciona una evaluación más precisa del desgaste de la muestra. Más allá de los métodos de ensayo tradicionales, la adopción de la cartografía de desgaste progresivo ha contribuido a importantes avances en el campo de los ensayos de suelos.

El tribómetro NANOVEA T2000 con perfilómetro 3D sin contacto integrado es una solución innovadora para pruebas de desgaste y mediciones de pérdida de volumen. Su capacidad para moverse con precisión entre el perno y el perfilómetro garantiza la fiabilidad de los resultados al eliminar cualquier desviación en el radio o la ubicación de la pista de desgaste. Pero eso no es todo: las funciones avanzadas del perfilómetro 3D sin contacto permiten realizar mediciones de superficies a alta velocidad, reduciendo el tiempo de exploración a unos segundos. Con capacidad para aplicar cargas de hasta 2.000 N y alcanzar velocidades de giro de hasta 5.000 rpm, el NANOVEA T2000 Tribómetro ofrece versatilidad y precisión en el proceso de evaluación. Está claro que este equipo desempeña un papel vital en la cartografía del desgaste progresivo.

 
pruebas de desgaste de suelos con tribómetro
pruebas de desgaste de suelos con perfilómetro

FIGURA 1: Montaje de la muestra antes de la prueba de desgaste (izquierda) y perfilometría de la huella de desgaste tras la prueba de desgaste (derecha).

OBJETIVO DE MEDICIÓN

Se realizaron pruebas de mapeo de desgaste progresivo en dos tipos de materiales para suelos: piedra y madera. Cada muestra se sometió a un total de 7 ciclos de prueba, con duraciones de prueba crecientes de 2, 4, 8, 20, 40, 60 y 120 s, lo que permitió comparar el desgaste a lo largo del tiempo. Después de cada ciclo de prueba, se perfiló la pista de desgaste utilizando el perfilómetro sin contacto NANOVEA 3D. A partir de los datos recogidos por el perfilómetro, se puede analizar el volumen del agujero y la tasa de desgaste utilizando las funciones integradas en el software NANOVEA Tribometer o nuestro software de análisis de superficies, Mountains.

NANOVEA T2000 Alta carga
Tribómetro neumático

LAS MUESTRAS

muestras de ensayo de cartografía de desgaste madera y piedra

PARÁMETROS DE LA PRUEBA DE CARTOGRAFÍA DE DESGASTE

CARGAR40 N
DURACIÓN DE LA PRUEBAvaría
VELOCIDAD200 rpm
RADIUS10 mm
DISTANCIAvaría
MATERIAL DE LA BOLACarburo de tungsteno
DIÁMETRO DE LA BOLA10 mm

La duración de la prueba utilizada en los 7 ciclos fue 2, 4, 8, 20, 40, 60 y 120 segundosrespectivamente. Las distancias recorridas fueron 0,40, 0,81, 1,66, 4,16, 8,36, 12,55 y 25,11 metros.

RESULTADOS DE LA CARTOGRAFÍA DEL DESGASTE

Suelos de madera

Ciclo de pruebasCOF máximoMín COFAvg. COF
10.3350.1240.275
20.3370.2070.295
30.3800.2290.329
40.3930.2650.354
50.3520.2050.314
60.3450.1990.312
70.3150.2110.293

 

ORIENTACIÓN RADIAL

Ciclo de pruebasPérdida de volumen total (µm3Distancia total
Recorrido (m)
Índice de desgaste
(mm/Nm) x10-5
Índice de desgaste instantáneo
(mm/Nm) x10-5
12962476870.401833.7461833.746
23552452271.221093.260181.5637
35963713262.88898.242363.1791
48837477677.04530.629172.5496
5120717995115.40360.88996.69074
6147274531827.95293.32952.89311
7185131921053.06184.34337.69599
índice de desgaste progresivo de la madera frente a la distancia total
Índice de desgaste del suelo de madera

FIGURA 2: Índice de desgaste frente a la distancia total recorrida (izquierda)
e índice de desgaste instantáneo frente al ciclo de ensayo (derecha) para suelos de madera.

pruebas del coeficiente de fricción del suelo
cartografía del desgaste progresivo del suelo de madera

FIGURA 3: Gráfico COF y vista 3D de la huella de desgaste de la prueba #7 en suelo de madera.

mapa de desgaste perfil extraído
resultados de las pruebas de desgaste de suelos
caracterización de la superficie del suelo

FIGURA 4: Análisis transversal de la pista de desgaste de madera del ensayo #7

mapeo progresivo del desgaste análisis de volumen y área

FIGURA 5: Análisis de volumen y área de la huella de desgaste en la muestra de madera Ensayo #7.

RESULTADOS DE LA CARTOGRAFÍA DEL DESGASTE

Suelos de piedra

Ciclo de pruebasCOF máximoMín COFAvg. COF
10.2490.0350.186
20.3490.1970.275
30.2940.1540.221
40.5030.1240.273
50.5480.1060.390
60.5100.1290.434
70.5270.1810.472

 

ORIENTACIÓN RADIAL

Ciclo de pruebasPérdida de volumen total (µm3Distancia total
Recorrido (m)
Índice de desgaste
(mm/Nm) x10-5
Índice de desgaste instantáneo
(mm/Nm) x10-5
1962788460.40595.957595.9573
28042897311.222475.1852178.889
313161478552.881982.355770.9501
431365302157.041883.2691093.013
51082173218015.403235.1802297.508
62017496034327.954018.2821862.899
74251206342053.064233.0812224.187
índice de desgaste de los suelos de piedra frente a la distancia
tabla de desgaste instantáneo de los suelos de piedra

FIGURA 6: Índice de desgaste frente a la distancia total recorrida (izquierda)
e índice de desgaste instantáneo frente al ciclo de ensayo (derecha) para suelos de piedra.

pruebas tribológicas de desgaste de suelos
suelo de piedra 3d perfil de la pista de desgaste

FIGURA 7: Gráfico COF y vista 3D de la huella de desgaste de la prueba #7 sobre pavimento de piedra.

suelo de piedra mapeo de desgaste progresivo perfil extraído
suelo de piedra perfil extraído profundidad y altura máximas área del agujero y pico
pruebas tribológicas de suelos

FIGURA 8: Análisis transversal de la huella de desgaste de piedra de la prueba #7.

análisis volumétrico de la cartografía de desgaste progresivo de los suelos de madera

FIGURA 9: Análisis de volumen y área de la huella de desgaste en la muestra de piedra de ensayo #7.

DEBATE

El índice de desgaste instantáneo se calcula con la siguiente ecuación:
fórmula de desgaste progresivo del suelo

Donde V es el volumen de un agujero, N es la carga y X es la distancia total, esta ecuación describe la tasa de desgaste entre ciclos de prueba. La tasa de desgaste instantánea puede utilizarse para identificar mejor los cambios en la tasa de desgaste a lo largo de la prueba.

Ambas muestras tienen comportamientos de desgaste muy diferentes. Con el tiempo, el suelo de madera comienza con un índice de desgaste elevado, pero desciende rápidamente a un valor más pequeño y constante. En el caso del suelo de piedra, el índice de desgaste parece comenzar con un valor bajo y tiende a aumentar con el paso de los ciclos. El índice de desgaste instantáneo también muestra poca consistencia. La razón específica de esta diferencia no es segura, pero puede deberse a la estructura de las muestras. El suelo de piedra parece estar formado por partículas sueltas similares al grano, que se desgastarían de forma diferente en comparación con la estructura compacta de la madera. Sería necesario realizar más pruebas e investigaciones para determinar la causa de este comportamiento de desgaste.

Los datos del coeficiente de fricción (COF) parecen concordar con el comportamiento de desgaste observado. El gráfico del COF para el suelo de madera parece coherente a lo largo de los ciclos, complementando su tasa de desgaste constante. En el caso de los suelos de piedra, el COF medio aumenta a lo largo de los ciclos, de forma similar a como lo hace la tasa de desgaste. También hay cambios aparentes en la forma de los gráficos de fricción, lo que sugiere cambios en la forma en que la bola interactúa con la muestra de piedra. Esto es más evidente en los ciclos 2 y 4.

CONCLUSIÓN

El Tribómetro NANOVEA T2000 muestra su capacidad para realizar un mapeo de desgaste progresivo analizando la tasa de desgaste entre dos muestras de pavimento diferentes. Detener la prueba de desgaste continuo y escanear la superficie con el perfilómetro sin contacto NANOVEA 3D proporciona información valiosa sobre el comportamiento de desgaste del material con el tiempo.

El tribómetro NANOVEA T2000 con el perfilómetro 3D sin contacto integrado proporciona una amplia variedad de datos, incluyendo datos COF (Coeficiente de Fricción), mediciones de superficie, lecturas de profundidad, visualización de superficie, pérdida de volumen, tasa de desgaste y más. Este amplio conjunto de información permite a los usuarios obtener una comprensión más profunda de las interacciones entre el sistema y la muestra. Con su carga controlada, alta precisión, facilidad de uso, alta carga, amplio rango de velocidad y módulos ambientales adicionales, el tribómetro NANOVEA T2000 lleva la tribología al siguiente nivel.

Inspección de mapas de rugosidad mediante perfilometría 3D

INSPECCIÓN CARTOGRÁFICA DE LA RUGOSIDAD

UTILIZANDO LA PERFILOMETRÍA 3D

Preparado por

DUANJIE, Doctor

INTRODUCCIÓN

La rugosidad y la textura de la superficie son factores críticos que influyen en la calidad final y el rendimiento de un producto. Un conocimiento profundo de la rugosidad, textura y consistencia de las superficies es esencial para seleccionar las mejores medidas de procesamiento y control. La inspección en línea rápida, cuantificable y fiable de las superficies de los productos es necesaria para identificar a tiempo los productos defectuosos y optimizar las condiciones de la línea de producción.

IMPORTANCIA DEL PERFILOMETRO 3D SIN CONTACTO PARA LA INSPECCION EN LINEA DE SUPERFICIES

Los defectos superficiales de los productos son el resultado del procesamiento de los materiales y la fabricación de los productos. La inspección en línea de la calidad de las superficies garantiza el más estricto control de calidad de los productos finales. NANOVEA Perfiladores ópticos 3D sin contacto utilizan la tecnología de luz cromática con una capacidad única para determinar la rugosidad de una muestra sin contacto. El sensor lineal permite escanear el perfil 3D de una gran superficie a gran velocidad. El umbral de rugosidad, calculado en tiempo real por el software de análisis, sirve como herramienta rápida y fiable de pasa/no pasa.

OBJETIVO DE MEDICIÓN

En este estudio, el NANOVEA ST400 equipado con un sensor de alta velocidad se utiliza para inspeccionar la superficie de una muestra de Teflon con defecto para mostrar la capacidad de NANOVEA

Profilómetros sin contacto en proporcionar una inspección de superficies rápida y fiable en una línea de producción.

NANOVEA

ST400

RESULTADOS Y DEBATE

Análisis tridimensional de la superficie del Rugosidad Muestra estándar

La superficie de un patrón de rugosidad se escaneó utilizando un NANOVEA ST400 equipado con un sensor de alta velocidad que genera una línea brillante de 192 puntos, como se muestra en la FIGURA 1. Estos 192 puntos escanean la superficie de la muestra al mismo tiempo, lo que conlleva un aumento significativo de la velocidad de escaneado.

La FIGURA 2 muestra vistas en falso color del Mapa de Altura de la Superficie y del Mapa de Distribución de la Rugosidad de la Muestra Estándar de Rugosidad. En la FIGURA 2a, el Estándar de Rugosidad exhibe una superficie ligeramente inclinada como se representa por el gradiente de color variado en cada uno de los bloques de rugosidad estándar. En la FIGURA 2b, se muestra una distribución homogénea de la rugosidad en differentes bloques de rugosidad, cuyo color representa la rugosidad en los bloques.

La FIGURA 3 muestra ejemplos de los mapas de aprobado/no aprobado generados por el software de análisis en función de diferentes umbrales de rugosidad. Los bloques de rugosidad se resaltan en rojo cuando su rugosidad superficial está por encima de un determinado valor umbral establecido. Esto proporciona una herramienta para que el usuario establezca un umbral de rugosidad para determinar la calidad del acabado superficial de una muestra.

FIGURA 1: Barrido del sensor óptico de líneas en la muestra del patrón de rugosidad

a. Mapa de altura de la superficie:

b. Mapa de rugosidad:

FIGURA 2: Vistas en falso color del Mapa de Altura de Superficie y del Mapa de Distribución de Rugosidad de la Muestra Estándar de Rugosidad.

FIGURA 3: Mapa Pasa/Falla basado en el Umbral de Rugosidad.

Inspección superficial de una muestra de Teflon con defectos

En la FIGURA 4 se muestran el mapa de altura de la superficie, el mapa de distribución de la rugosidad y el mapa de umbral de rugosidad Pasa/Falla de la superficie de la muestra de Teflon. La muestra de Teflon presenta una cresta en el centro derecho de la muestra, como se muestra en el mapa de altura de la superficie.

a. Mapa de altura de la superficie:

Los differentes colores de la paleta de la FIGURA 4b representan el valor de rugosidad en la superficie local. El mapa de rugosidad muestra una rugosidad homogénea en la zona intacta de la muestra de Teflon. Sin embargo, los defectos, en las formas de un anillo indentado y una cicatriz de desgaste se destacan en color brillante. El usuario puede configurar fácilmente un umbral de rugosidad Pasa/Falla para localizar los defectos superficiales, como se muestra en la FIGURA 4c. Esta herramienta permite a los usuarios supervisar in situ la calidad de la superficie del producto en la línea de producción y descubrir a tiempo los productos defectuosos. El valor de rugosidad en tiempo real se calcula y registra a medida que los productos pasan por el sensor óptico en línea, lo que puede servir como una herramienta rápida pero fiable para el control de calidad.

b. Mapa de rugosidad:

c. Mapa de umbrales de rugosidad Pasa/Falla:

FIGURA 4: Mapa de altura de la superficie, mapa de distribución de la rugosidad y Mapa de umbral de rugosidad Pasa/Falla de la superficie de la muestra de Teflon.

CONCLUSIÓN

En esta aplicación, hemos demostrado cómo el perfilador óptico sin contacto 3D NANOVEA ST400 equipado con un sensor óptico de línea funciona como una herramienta de control de calidad fiable de manera eficaz y eficiente.

El sensor óptico de línea genera una línea brillante de 192 puntos que escanean la superficie de la muestra al mismo tiempo, lo que aumenta significativamente la velocidad de escaneado. Puede instalarse en la línea de producción para controlar in situ la rugosidad de la superficie de los productos. El umbral de rugosidad funciona como un criterio fiable para determinar la calidad de la superficie de los productos, lo que permite a los usuarios detectar a tiempo los productos defectuosos.

Los datos mostrados aquí representan sólo una parte de los cálculos disponibles en el software de análisis. Los perfilómetros NANOVEA miden prácticamente cualquier superficie en campos como los semiconductores, la microelectrónica, la energía solar, la fibra óptica, la automoción, la industria aeroespacial, la metalurgia, el mecanizado, los revestimientos, la industria farmacéutica, la biomedicina, el medio ambiente y muchos otros.

Inspección de superficies soldadas con un perfilómetro 3D portátil

Inspección de superficies soldadas

utilizando un perfilómetro 3D portátil

Preparado por

CRAIG LEISING

INTRODUCCIÓN

Puede ser fundamental que una soldadura concreta, normalmente inspeccionada visualmente, se examine con un nivel extremo de precisión. Las áreas específicas de interés para un análisis preciso incluyen las grietas superficiales, la porosidad y los cráteres sin rellenar, independientemente de los procedimientos de inspección posteriores. Las características de la soldadura, como la dimensión/forma, el volumen, la rugosidad, el tamaño, etc., pueden medirse para realizar una evaluación crítica.

IMPORTANCIA DEL PERFILÓMETRO 3D SIN CONTACTO PARA LA INSPECCIÓN DE SUPERFICIES SOLDADAS

A diferencia de otras técnicas, como las sondas táctiles o la interferometría, el NANOVEA Perfilómetro 3D sin contacto, mediante el cromatismo axial, puede medir casi cualquier superficie, los tamaños de las muestras pueden variar ampliamente debido a la disposición abierta y no es necesario preparar las muestras. Se obtiene un rango de nano a macro durante la medición del perfil de la superficie sin influencia alguna de la reflectividad o absorción de la muestra, tiene una capacidad avanzada para medir ángulos de superficie elevados y no hay manipulación de los resultados por parte del software. Mida fácilmente cualquier material: transparente, opaco, especular, difusivo, pulido, rugoso, etc. Las capacidades 2D y 2D de los perfilómetros portátiles NANOVEA los convierten en instrumentos ideales para la inspección completa de la superficie de soldadura, tanto en el laboratorio como en el campo.

OBJETIVO DE MEDICIÓN

En esta aplicación, se utiliza el perfilómetro portátil NANOVEA JR25 para medir la rugosidad de la superficie, la forma y el volumen de una soldadura, así como el área circundante. Esta información puede proporcionar datos fundamentales para investigar adecuadamente la calidad de la soldadura y el proceso de soldadura.

NANOVEA

JR25

RESULTADOS DE LAS PRUEBAS

La imagen siguiente muestra la vista 3D completa de la soldadura y la zona circundante, junto con los parámetros superficiales de la soldadura únicamente. A continuación se muestra el perfil de la sección transversal en 2D.

la muestra

Una vez eliminado el perfil transversal 2D anterior del 3D, se calcula la información dimensional de la soldadura a continuación. Área superficial y volumen del material calculados solo para la soldadura a continuación.

 AGUJEROMÁXIMO
SUPERFICIE1,01 mm214,0 mm2
VOLUMEN8,799e-5 mm323,27 mm3
PROFUNDIDAD/ALTURA MÁXIMA0,0276 mm0,6195 mm
PROFUNDIDAD/ALTURA MEDIA 0,004024 mm 0,2298 mm

CONCLUSIÓN

En esta aplicación, hemos mostrado cómo el perfilómetro sin contacto NANOVEA 3D puede caracterizar con precisión las características críticas de una soldadura y la superficie circundante. A partir de la rugosidad, las dimensiones y el volumen, se puede determinar y/o investigar más a fondo un método cuantitativo para la calidad y la repetibilidad. Las soldaduras de muestra, como el ejemplo de esta nota de aplicación, se pueden analizar fácilmente con un perfilómetro NANOVEA de mesa estándar o portátil para pruebas internas o de campo.