USA/GLOBAL: +1-949-461-9292
EUROPA: +39-011-3052-794
KONTAKT US

Kategorie: Profilometrische Prüfung

 

Soft and transparent materials including a biomedical membrane, microfluidic device, and wearable sensor for non-contact profilometry applications

Non-Contact Profilometry of Soft and Transparent Materials

Application Note | Non-Contact 3D Profilometry

Non-Contact Profilometry of Soft and Transparent Materials

Comprehensive Characterization of Challenging Surfaces Without Contact, Deformation, or Sample Preparation

Examples of soft and transparent material applications for non-contact profilometry, including biomedical membranes, microfluidics, and wearable sensors

Research & Experimental Testing

Craig Leising

Visual Design & Editorial

Andrew Shore

Einführung

Soft, transparent, and easily deformable materials are increasingly important across advanced applications including flexible bioelectronics, wearable sensors, biomedical interfaces, microfluidic devices, and other polymer-based technologies. Characterizing these materials can be difficult because the measurement method itself may influence the surface or fail to capture it reliably.

Contact-based techniques can deform, scratch, or move soft materials during measurement, while transparent or absorptive surfaces can present additional challenges for some optical techniques. Non-contact profilometry avoids physical interaction with the sample while enabling quantitative surface characterization across challenging material types.

In this study, an extremely soft and translucent petroleum-jelly-based material was selected as a demanding proof-of-concept sample. Using the NANOVEA ST400 Profilometer, the surface was characterized without physical contact or sample preparation to demonstrate the broader capability of non-contact profilometry for delicate and difficult-to-measure materials.

The Advantage of Non-Contact Profilometry for Challenging Materials

Soft materials can be difficult to measure accurately because physical contact may alter the surface during the measurement itself. Films, gels, and other compliant materials can deform, scratch, or move under a contacting probe, potentially changing the geometry being characterized.

Transparent and absorptive surfaces can introduce additional measurement challenges for some optical techniques, including effects associated with light transmission, absorption, and internal reflections. NANOVEA Non-Contact Profilometers use axial chromatism to determine surface height without physically contacting the sample.

This combination enables quantitative characterization of challenging surfaces while minimizing measurement influence. Depending on the application, measurements can include surface roughness, flatness, 3D topography, surface area, profile geometry, and other dimensional characteristics without requiring sample preparation.

Messung Zielsetzung

The objective of this study was to demonstrate non-contact surface characterization on an extremely soft and translucent material, representing the type of measurement challenge encountered when a surface may be altered by physical contact or prove difficult for some optical techniques.

A petroleum-jelly-based lip balm was selected as a deliberately challenging proof-of-concept sample because of its softness and translucency. The sample was measured using the NANOVEA ST400 Profilometer without physical contact or sample preparation.

The resulting measurement was used to obtain 3D topography, 2D profile data, surface roughness, flatness, and 3D surface area, demonstrating the range of quantitative surface information that can be obtained from a delicate material using non-contact profilometry.

NANOVEA ST400 Non-Contact

Optisches Profilometer

Optical Profilometry Results

Soft transparent petroleum-jelly-based lip balm sample used for non-contact profilometry

Soft, translucent petroleum-jelly-based sample used for non-contact profilometry.

Soft transparent petroleum-jelly-based sample positioned under the NANOVEA ST400 profilometer for non-contact surface measurement

The sample being scanned by the NANOVEA ST400 for non-contact surface measurement.

3D Profile Measurement

The NANOVEA ST400 captured the 3D surface of the extremely soft and translucent sample without physically contacting the material. The resulting topography was used to evaluate multiple aspects of the surface, including ISO 25178 surface parameters, 3D surface area, and flatness corresponding to ISO 12781. A 2D cross-section was also extracted from the measurement to provide additional profile detail.

Obtaining these measurements from such a soft and translucent surface demonstrates the value of non-contact profilometry for materials that could otherwise be altered by a contacting probe or present challenges for some optical techniques. Quantitative surface geometry can be acquired while preserving the condition of the measured surface.

3D non-contact profilometry measurement of a soft transparent petroleum-jelly-based sample with ISO 25178 surface parameters

3D surface profile of the soft, transparent sample with ISO 25178 surface parameters and flatness analysis.

2D Profile Measurement

2D profile extracted from non-contact profilometry of a soft transparent petroleum-jelly-based sample

2D profile extracted from the non-contact 3D surface measurement across a 4 mm section of the sample.

An intensity/contrast image was also acquired simultaneously with the 3D surface measurement, providing complementary visual information alongside the measured topography.

False-color height map from non-contact profilometry of a soft transparent petroleum-jelly-based sample

False-color height map showing surface height variation across the soft, translucent sample.

Intensity image acquired during non-contact profilometry of a soft transparent petroleum-jelly-based sample

Intensity image acquired simultaneously with the 3D surface measurement.

Schlussfolgerung

This study demonstrates how non-contact profilometry can characterize surfaces that combine two particularly difficult measurement conditions: extreme softness and translucency. Using the NANOVEA ST400, quantitative 3D surface data were acquired without physically contacting or preparing the sample.

A petroleum-jelly-based lip balm was selected as a deliberately challenging proof-of-concept material rather than as the end application itself. Its soft, translucent surface provided a practical demonstration of the ability to obtain surface roughness, flatness, 3D surface area, profile geometry, and complementary intensity data while minimizing the influence of the measurement process on the surface.

This capability is relevant wherever delicate, compliant, transparent, or absorptive materials must be characterized without deformation or surface damage. As soft polymers, gels, transparent elastomers, and related materials continue to appear in areas such as biomedical interfaces, wearable technologies, microfluidics, and advanced polymer systems, non-contact surface measurement provides a useful approach for evaluating their surface geometry and topography.

Frequently Asked Questions About Non-Contact Profilometry

Why is non-contact profilometry useful for soft materials?

Soft materials can deform, scratch, or move when touched by a contacting probe. Non-contact profilometry measures the surface optically, reducing the risk that the measurement itself alters the geometry being characterized.

Can non-contact profilometry measure transparent materials?

Yes, depending on the optical technology and material. NANOVEA profilometers use axial chromatism to determine surface height and can characterize transparent, opaque, specular, diffusive, polished, and rough surfaces without physical contact.

Can soft and transparent surfaces be measured without sample preparation?

In this study, the soft and transparent petroleum-jelly-based sample was measured without sample preparation. Avoiding coatings or other surface modification can be especially valuable when the original surface condition needs to be preserved.

What can be measured with non-contact 3D profilometry?

Non-contact 3D profilometry can provide quantitative measurements including surface roughness, 3D topography, flatness, surface area, 2D profiles, and other dimensional characteristics, depending on the measurement objective and surface geometry.

What types of materials benefit from non-contact surface measurement?

Non-contact measurement is especially useful for materials that are soft, delicate, transparent, semi-transparent, easily scratched, or otherwise difficult to probe physically. It can also be useful when maintaining the original surface condition is important.

How is non-contact profilometry different from contact profilometry?

Contact profilometry uses a physical stylus that moves across the surface. Non-contact profilometry acquires surface height optically, eliminating probe-to-sample contact and reducing the possibility of contact-induced deformation, scratching, or movement on sensitive materials.

Pacemaker and endocardial pacing leads shown in a translucent medical illustration for pacing lead insulation wear testing

Pacing Lead Insulation Wear Testing in Hanks’ Solution

Application Note | Medical Device Tribology

Nano-Friction and Wear Testing of Pacing Lead Insulation in Hanks’ Solution

Tribological analysis of silicone and polyether-polyurethane endocardial lead materials

Medical illustration of a pacemaker with two endocardial pacing leads routed into the heart for pacing lead insulation wear testing context

Research & Experimental Testing

Duanjie Li, PhD

Visual Design & Editorial

Andrew Shore

Einführung

A pacemaker is a medical device used to regulate heart rhythm and maintain an adequate heart rate. It is typically implanted in the chest or abdomen and sends electrical impulses to the heart muscle through endocardial pacing leads.

As pacemakers remain a widely used treatment for cardiac rhythm disorders, the quality and service life of pacing leads are critical to long-term device performance. Lead failures can create serious risks for patients and may require surgical replacement, making pacing lead insulation wear testing an important part of material evaluation for implantable cardiac devices.1–5
Endocardial pacing leads with insulated lead bodies used in implantable cardiac devices

Endocardial pacing leads transmit electrical impulses from a pacemaker to the heart while operating in a dynamic body-fluid environment.

Why Friction and Wear Matter for Endocardial Lead Insulation

The outer insulation material of an endocardial lead requires several key properties, including biological inertness, high flexibility, fracture toughness, and long service life. Low friction can reduce interaction between the lead and the blood vessel, helping minimize vessel irritation during implantation and movement.

Wear resistance is also critical. Endocardial leads experience continuous movement from the heart and surrounding body structures, while operating in a body-fluid environment that can influence friction, wear, and material response.

Because of this complex environment, endocardial lead insulation should be evaluated using controlled tribological methods that simulate relevant contact conditions. Testing in Hanks’ solution allows the friction and wear behavior of lead insulation materials to be compared under a simulated body-fluid condition rather than relying only on dry testing.

Nano-friction test setup for measuring pacing lead insulation materials in Hanks’ solution

Nano-friction test setup used to evaluate endocardial pacing lead insulation materials under low-load contact conditions.

Messung Zielsetzung

This study compares the nano-friction and wear behavior of endocardial pacing lead insulation materials in Hanks’ solution. Silicone and polyether-polyurethane lead materials were evaluated to determine how each material responds under simulated body-fluid conditions.

Low-load nano-friction testing was performed using the Nano Module of the NANOVEA Mechanischer Tester to measure coefficient of friction at controlled contact force. Reciprocating wear testing was then performed using a NANOVEA Tribometer to compare wear resistance under linear sliding contact.

NANOVEA T50 Kompakt
Tribometer mit freiem Gewicht

NANOVEA PB1000 Große Plattform Mechanischer Tester

Measurement Principle

Nano-Friction Measurement Principle

Nano-friction testing measures the coefficient of friction (COF) between the test surface and a controlled counter material under very low applied load. In this study, the indenter made contact with the pacing lead insulation surface while the Nano Module maintained a constant load throughout the measurement.

The Nano Module uses a fast piezoelectric system and load cell to adjust the ball position and keep the applied load stable during sliding. The sample is moved at a controlled speed while lateral force is measured and plotted against displacement.

A stainless steel ball with a 6 mm diameter is commonly used for this type of measurement, although other counter materials, shapes, and sizes can be selected to simulate different contact conditions. This allows pacing lead insulation materials to be evaluated under controlled low-load friction conditions relevant to biomedical device applications.

Schematic of the nano-friction measurement principle showing a ball-tip indenter under controlled constant load, a capacitive depth sensor, non-destructive load, and reciprocating sample motion on a friction spring table

Nano-friction measurement schematic showing controlled low-load sliding contact and lateral force measurement during reciprocating motion.

Reciprocating Wear Principle

Reciprocating wear testing evaluates material response under repeated linear sliding contact. A flat or spherical counter material is loaded against the test sample with a precisely known force, while the sample moves back and forth in a controlled reciprocating motion.

The counter material, such as a pin or ball, is mounted on a stiff lever that functions as a low-friction force transducer. As the sample moves, frictional forces between the counter material and the sample are measured using a strain gauge sensor on the tribometer arm.

After the test, the resulting wear track can be examined to compare material damage, wear scar geometry, and surface response. This method allows friction and wear behavior to be studied under controlled conditions, including variations in time, contact pressure, sliding speed, temperature, humidity, and lubrication environment.

Schematic of the reciprocating wear principle showing adjustable weights, tribometer arm, pin or ball holder, strain gauge, sample stage, linear wear track, and linear reciprocating motion

Linear reciprocating wear schematic showing a pin or ball counterface sliding across the sample to generate a wear track under controlled load.

Testverfahren

The coefficient of friction (COF) of the pacing lead materials was measured against a stainless steel 440 ball with a 6 mm diameter. Testing was performed using the Nano Module of the Nanovea Mechanical Tester.

The sample was immersed in Hanks’ solution to simulate a body-fluid environment. A low applied load of 50 mN was maintained throughout the test, while the ball slid against the lead surface at a constant speed of 20 mm/min over a total sliding distance of 10 mm.

Wear resistance was evaluated using a Nanovea Tribometer with the Linear Reciprocating Wear Module. During the wear test, a stainless steel 303 block measuring 10 × 10 mm² was used as the counter material, and the coefficient of friction was recorded in situ at 0.1 s intervals.

After testing, the resulting wear tracks were examined under an optical microscope to compare surface damage on the silicone and polyether-polyurethane lead materials. Stainless steel was used as the counter material in this study; however, custom fixtures and alternative counter materials can be used to simulate specific application conditions.

Parameter Value
Sample Leads made of silicone or polyether-polyurethane (PP)
Normal force 1 N
Geschwindigkeit 200 cycles/min
Duration of test 5 h
Umwelt Hanks’ solution

Wear test parameters used to evaluate silicone and polyether-polyurethane pacing lead materials in Hanks’ solution.

Ergebnisse und Diskussion

Nano-Friction Test

The nano-friction behavior of the silicone and polyether-polyurethane (PP) pacing lead materials was first evaluated using the Nano Module of the Nanovea Mechanical Tester. The coefficient of friction was measured in both dry conditions and Hanks’ solution to compare material response under ambient and simulated body-fluid environments.

Both materials showed significantly lower coefficient of friction in Hanks’ solution than under dry conditions. In Hanks’ solution, the silicone lead exhibited a COF of approximately 0.15, while the polyether-polyurethane lead exhibited a lower COF of approximately 0.05. Under dry conditions, the values were substantially higher, at approximately 0.6 for silicone and 0.5 for polyether-polyurethane.

These results demonstrate the importance of testing pacing lead insulation materials under application-relevant environmental conditions. Hanks’ solution had a strong effect on the measured friction behavior, showing that dry testing alone may not represent the tribological response of lead insulation materials in a simulated body-fluid environment.

The low-load control of the Nano Module allowed the applied force to remain constant at 50 mN during the measurement. This enabled controlled simulation of low-contact-force interaction between the lead material and surrounding biological structures.

Graph comparing coefficient of friction of silicone and polyether-polyurethane pacing lead materials in dry conditions and Hanks’ solution

Coefficient of friction comparison for silicone and polyether-polyurethane pacing lead materials in dry conditions and Hanks’ solution.

Wear Test

Wear resistance was evaluated using a Nanovea Tribometer to compare the silicone and polyether-polyurethane pacing lead materials in Hanks’ solution. After testing, the lead surfaces were examined visually and under optical microscopy to compare the extent of wear damage.

The silicone lead showed a large wear scar with a width of approximately 1.2 mm. Microscopic observation indicated severe wear on the silicone lead, with parallel deep grooves formed along the movement direction of the rubbing block.

In comparison, the polyether-polyurethane lead showed a narrower wear scar of approximately 0.6 mm. The observed wear was milder, with only several small scratches visible on the shallow surface.

Wear of the lead outer insulation can contribute to pacing and sensing abnormalities, making wear resistance an important factor in endocardial lead material selection.6 These results indicate that polyether-polyurethane provided lower friction and better wear resistance than silicone under the tested conditions.

Before-and-after wear comparison of silicone and polyether-polyurethane pacing lead surfaces, including 400x microscope images showing more severe wear on silicone and milder wear on polyether-polyurethane.

Silicone pacing lead surface before wear testing in Hanks’ solution

Silicone pacing lead surface before reciprocating wear testing.

Polyether-polyurethane pacing lead surface before wear testing in Hanks’ solution

Polyether-polyurethane pacing lead surface before reciprocating wear testing.

Silicone pacing lead surface after wear testing showing a large wear scar

Silicone pacing lead surface after wear testing, showing a pronounced wear scar.

Polyether-polyurethane pacing lead surface after wear testing showing a smaller wear scar

Polyether-polyurethane pacing lead surface after reciprocating wear testing.

Microscope image at 400x magnification showing severe wear grooves on silicone pacing lead surface

400x microscope image of the silicone pacing lead after wear testing, showing deep parallel wear grooves.

Microscope image at 400x magnification showing mild wear on polyether-polyurethane pacing lead surface

400x microscope image of the polyether-polyurethane pacing lead after wear testing, showing comparatively mild surface wear.

Schlussfolgerung

This study demonstrated the use of low-load nano-friction testing and reciprocating wear testing to evaluate endocardial pacing lead insulation materials in Hanks’ solution. The Nano Module of the NANOVEA Mechanical Tester measured coefficient of friction under controlled low-load contact, while the NANOVEA Tribometer simulated wear behavior under reciprocating sliding motion.

Testing in Hanks’ solution showed a clear difference between silicone and polyether-polyurethane lead materials. Polyether-polyurethane exhibited lower coefficient of friction and better wear resistance than silicone under the tested conditions, making it the stronger candidate for the outer insulation material of endocardial pacing leads in this study.

These results highlight the importance of evaluating biomedical materials under application-relevant environments rather than relying only on dry testing. Controlled nano-friction and tribology testing can help compare candidate materials, quantify friction response, and evaluate wear resistance for implantable medical device components.

The NANOVEA Mechanical Tester’s Nano, Micro, and Macro modules operate within a single ISO and ASTM compliant platform, enabling consistent evaluation of hardness, elastic modulus, fracture toughness, and wear from a single system. The NANOVEA Tribometer similarly supports rotative and linear wear modes with optional high-temperature, corrosion, and liquid environment modules.

Referenzen

[1] Magney JE, Flynn DM, Parsons JA, Staplin DH, Chin-Purcell MV, Milstein S, Hunter DW. Pacing Clin Electrophysiol. 1993; 16:445–457.
[2] Jacobs DM, Fink AS, Miller RP, Anderson WR, McVenes RD, Lessar JF, Cobian KE, et al. Pacing Clin Electrophysiol. 1993; 16:434–444.
[3] Gupta K, Villareal RP, Rasekh A, Massumi A. Tex Heart Inst J. 2003; 30:84–85.
[4] Magney JE, Parsons JA, Flynn DM, Hunter DW. Pacing Clin Electrophysiol. 1995; 18:1509–1517.
[5] Kazama S, Nishiyama K, Machii M, Tanaka K, Amano T, Nomura T, Ohuchi M, et al. Jpn Heart J. 1993; 34:193–200.
[6] Andrzej K, Barbara M, Agnieszka K, Marcin G. Pacing Clin Electrophysiol. 2013; 36(12):1503–1511.

Frequently Asked Questions About Pacing Lead Insulation Wear Testing

How do you evaluate friction and wear behavior of pacing lead insulation?

Pacing lead insulation can be evaluated using low-load friction testing and reciprocating wear testing. These methods measure coefficient of friction, wear scar formation, and surface damage under controlled load, motion, and environmental conditions.

Why is low-load friction testing important for endocardial leads?

Endocardial leads operate under relatively low contact forces while interacting with blood vessels, tissue, and surrounding structures. Low-load friction testing helps evaluate how insulation materials behave under contact conditions that are closer to the application than high-force mechanical testing alone.

What does coefficient of friction indicate in pacing lead material testing?

Coefficient of friction indicates how much resistance occurs during sliding contact between the lead insulation and a counter material. In this study, lower COF values in Hanks’ solution showed that the test environment had a strong effect on the measured friction behavior of silicone and polyether-polyurethane materials.

Why compare silicone and polyether-polyurethane lead insulation materials?

Silicone and polyether-polyurethane are commonly considered for flexible biomedical insulation applications because they can provide different combinations of flexibility, durability, and surface response. Comparing them under the same test conditions helps identify which material provides lower friction and better wear resistance for the intended application.

Which NANOVEA instruments are used for low-load friction and wear testing?

Low-load coefficient of friction can be measured using the Nano Module of a NANOVEA Mechanical Tester, while reciprocating wear behavior can be evaluated using a NANOVEA Tribometer. Together, these systems allow controlled evaluation of friction, wear, and material response for biomedical components.

How is reciprocating wear testing used for pacing lead materials?

Reciprocating wear testing repeatedly slides a counter material across the sample surface under controlled load to create and evaluate a wear track. For pacing lead insulation materials, this allows comparison of wear scar width, surface damage, and material durability under simulated sliding contact.

Need Reliable Medical Device Friction and Wear Testing?

3D optical profilometry image showing climbing hold surface roughness, pore morphology, and grip-related texture features.

Climbing Hold Surface Roughness Analysis

Application Note | 3D Optical Profilometry

Climbing Hold Surface Roughness Analysis Using 3D Optical Profilometry

Measuring Texture, Porosity, and Topography on Bouldering Holds

Bouldering holds analyzed for climbing hold surface roughness using 3D optical profilometry.

Research & Experimental Testing

Walter Alabiso, PhD

Visual Design & Editorial

Andrew Shore

Einführung

Bouldering is a demanding discipline that combines physical strength, precise body positioning, and an understanding of how the human body interacts with climbing surfaces. On slab routes, where the wall is angled below vertical and positive holds are limited or absent, a climber’s stability depends almost entirely on the tribological interaction between the body and the climbing hold surface.

Climbing hold surface roughness plays a central role in this contact. Roughness provides the microtexture needed for smearing, a technique where high-friction rubber soles are pressed firmly against the surface to expand the effective contact area and generate adherence. A similar mechanism occurs at the fingers, where the ridges of fingerprints and the pliability of skin deform slightly against the hold’s surface features, creating grip through microscopic interlocking.

Porosity contributes to grip performance by absorbing moisture, sweat, or chalk at the contact interface, preventing the formation of a thin lubricating film that would reduce friction. Micro-cracks and surface flaws act as additional friction points, helping the climber maintain lateral tension against the hold surface. Because these features (roughness, porosity, and surface morphology) operate at different scales and interact differently depending on the hold, quantitative 3D surface measurement is essential for comparing how different climbing hold textures perform under real contact conditions.

Bouldering grips used to compare surface roughness, pore morphology, and grip-related topography.

Why Use Non-Contact Profilometry for Climbing Hold Surface Analysis

Climbing holds and rock-like surfaces can include deep pores, steep asperities, sharp valleys, and irregular texture. These features are difficult to measure accurately with contact-based profilometry because a physical stylus can lose contact, deform local surface features, or fail to reach narrow cavities.

NANOVEA’s non-contact optical profilometry uses chromatic light technology to capture surface height data without touching the sample. This makes it suitable for reconstructing complex climbing hold topography, including deep nooks, pores, and surface flaws, while avoiding measurement artifacts caused by local plastic deformation.

In this study, the NANOVEA JR25 Optical Profiler was used to measure two bouldering grips: a yellow block with a smoother, flatter surface and a green block with a rougher tactile texture. Both samples were scanned using a PS4-MG35 single-point optical sensor with a 3000 µm Z-range and a 4 µm acquisition step in X and Y.

Dual-frequency acquisition was used to reduce light sensor saturation from localized bright spots on the grip surfaces, allowing the profiler to capture roughness and pore morphology across the scanned areas.

Messung Zielsetzung

The objective of this study was to demonstrate how non-contact 3D optical profilometry can be used to reconstruct and compare the surface roughness, topography, and pore morphology of climbing holds.

Two bouldering grip samples were analyzed: a yellow hold with a smoother, flatter surface and a blue hold with a rougher tactile texture and sharper grip features. The analysis focused on surface height variation, areal roughness parameters, pore coverage, pore size, pore depth, and functional surface behavior.

The NANOVEA JR25 Optical Profilometer measuring the climbing hold samples using an optical sensor.

Measurement Method

The NANOVEA JR25 Optical Profiler was used to measure the yellow and blue bouldering grip samples. Each surface was scanned with a PS4-MG35 single-point optical sensor with an enhanced 3000 µm Z-range, allowing the system to capture deep pores, sharp valleys, and irregular surface texture while maintaining a 4 µm acquisition step in X and Y.

Dual-frequency acquisition was used to reduce light sensor saturation from localized bright spots on the grip surfaces, improving data capture across rough, porous, and uneven areas.

NANOVEA JR25 Portable

Optisches Profilometer

Test-Parameter

Measurement Setting Optical Profilometry Setup
Samples measured Yellow and blue bouldering grip samples
Optical pen PS4-MG35
Z-range 3000 µm
Scan area 5.00 mm × 5.00 mm
X-step size 4.00 µm
Y-step size 4.00 µm
Averaging 1
Measurement type Direct
Acquisition mode Dual frequency
Acquisition rate 100–400 Hz
Light intensity 100%

Optical profilometry test conditions used to measure the bouldering grip samples.

Optical Profilometry Results

Yellow Grip Sample

Surface Roughness Analysis

The 3D rendering below shows the reconstructed surface topography of the yellow climbing grip sample.

3D optical profilometry reconstruction of the yellow climbing grip surface showing pores, roughness, and surface height variation.

A total least-squares plane was removed to study surface properties. The roughness filters S-Gaussian 2.5 µm was applied following ISO 25178 (1/2 cut-off removed at each side). However, the sharp density of pores and asperities and the elevated average roughness make the use of a Gaussian L-filter (8 mm cut off) inapplicable. Therefore, the primary surface was considered, and the roughness parameters are listed in the table below, alongside the 2D false-color map of the filtered surface.

False-color optical profilometry surface roughness map of the yellow climbing grip sample with ISO 25178 height parameters.
ISO 25178-2 – Primary Surface
S-filter (λs): Gaussian, 2.5 µm, 1/2 cut-off
F-operation: [Workflow] Leveled (TLSPL)
Height Parameters
Sq 168.970 µm Wurzel-Mittel-Quadrat-Höhe
Ssk -0.927 Schrägheit
Sku 4.117 Kurtosis
Sp 320.530 µm Maximale Peakhöhe
Sv 868.116 µm Maximum pit depth
Sz 1188.645 µm Maximale Höhe
Sa 132.953 µm Arithmetisches Mittel der Höhe

The average surface roughness Sa is 132.953 µm, whereas the peak-to-valley roughness, Sz amounts to 1188.645 µm. The surface morphology is skewed towards deep valleys (Ssk < 0, Sv > Sp), with a leptokurtotic (Sku > 3) distribution of peaks and valleys relative to the average plane.

The following picture shows a 2D photo-simulation of the area under artificial lighting, highlighting the region’s morphology.

2D photo simulation of the yellow climbing grip surface showing pores, roughness, and morphology under artificial lighting.

Pore Morphology Analysis

A pore analysis was performed across the full scanned area using a semi-automated edge-detection algorithm. The analysis identified recessed surface features to quantify pore coverage, pore density, radius, void volume, and maximum depth.

Pore detection analysis of the yellow climbing grip surface using semi-automated edge detection to identify recessed surface features.

The detected pore locations were then mapped across the scanned 5 mm × 5 mm area to evaluate pore coverage, density, and size distribution.

Pore distribution map of the yellow climbing grip sample showing detected recessed surface features across a 5 mm by 5 mm scanned area.
Information
MethodCircle detection
Features detectedPores, recessed objects
Minimum detection diameter0.150 mm
Maximum detection diameter2.000 mm
Number of detected pores206
Surface coverage47.395%
Pore density8.203 particles/mm²
Global Statistics
ParameterUnitMeanStd. Dev.MinMax
Radiusmm0.1270.0490.0760.275
Void volumeµm³4,724,770.7056,748,143.92523,594.1724.422 × 10⁷
Maximum depthµm173.72994.94228.153716.480

Pores covered nearly half of the yellow grip’s scanned surface, with a measured coverage of 47.395% and a pore density of 8.203 particles/mm². The detected pores and cracks were highly heterogeneous in size, volume, and depth, ranging from large crater-like features with a maximum radius of 0.275 mm and void volume above 4.4 × 10⁷ µm³ to smaller pores with a minimum radius of 0.076 mm and void volume of 23,594.172 µm³. This uneven pore distribution is reflected in the large standard deviation measured for void volume and maximum depth.

Functional Surface Parameters (Abbott-Firestone curve)

The Abbott-Firestone curve shows the cumulative areal material distribution of the yellow climbing grip sample. This analysis defines functional surface parameters including Sk, Spk, and Svk according to ISO 25178-2.

Abbott-Firestone curve for the yellow climbing grip sample showing cumulative areal material distribution and functional surface parameters.
Information
Standard ISO 25178-2
Parameter Value Unit
Sk 409.738 µm
Spk 45.480 µm
Svk 233.446 µm
Smrk1 3.976 %
Smrk2 85.005 %

The chart below shows the peak-valley distribution from the mean plane based on the functional parameters derived from the Abbott-Firestone curve. Valleys are shown in purple, the mean plane in green, and peaks in orange.

Peak-valley distribution map of the yellow climbing grip sample showing valleys, mean plane regions, and peaks derived from Abbott-Firestone functional parameters.
Information
1st threshold Height – c1: 229.209 µm
2nd threshold Height – c2: -180.424 µm
Parameters Unit
Projected area (in %) % 14.995 81.029 3.976
Projected area mm² 3.772 20.381 1.000
Volume of material (in %) % 97.451 48.100 0.973
Volume of material µm³ 1.684 × 10¹⁰ 4.956 × 10⁹ 2.275 × 10⁷

The yellow grip sample shows a dominant mean-plane region with scattered recessed pores and a smaller population of raised peaks. This indicates a surface texture characterized mainly by average-sized pores distributed across the scanned area.

Blue Grip Sample

Surface Roughness Analysis

The 3D rendering below shows the reconstructed surface topography of the blue climbing grip sample.

3D optical profilometry reconstruction of the blue climbing grip surface showing roughness, pores, asperities, and surface height variation.

A total least-squares plane was removed to evaluate the blue grip’s surface properties. An S-Gaussian 2.5 µm roughness filter was applied following ISO 25178, with 1/2 cut-off removed at each side.

Because of the dense pores, asperities, and elevated average roughness, a Gaussian L-filter with an 8 mm cut-off was not applied. The primary surface was used for roughness analysis, with the roughness parameters listed alongside the 2D false-color map of the filtered surface.

False-color optical profilometry surface roughness map of the blue climbing grip sample with ISO 25178 height parameters.
ISO 25178-2 – Primary Surface
S-filter (λs): Gaussian, 2.5 µm, 1/2 cut-off
F-operation: [Workflow] Leveled (TLSPL)
Height Parameters
Sq 211.440 µm Wurzel-Mittel-Quadrat-Höhe
Ssk -0.682 Schrägheit
Sku 3.672 Kurtosis
Sp 522.404 µm Maximale Peakhöhe
Sv 720.164 µm Maximum pit depth
Sz 1242.568 µm Maximale Höhe
Sa 166.719 µm Arithmetisches Mittel der Höhe

The blue grip sample had an average surface roughness, Sa, of 166.719 µm and a peak-to-valley roughness, Sz, of 1242.568 µm. The negative skewness value, Ssk &lt; 0, indicates that the surface morphology is skewed toward deep valleys, while Sv &gt; Sp shows that the maximum pit depth exceeded the maximum peak height.

The kurtosis value, Sku &gt; 3, indicates a leptokurtotic height distribution, meaning the blue grip surface contains sharper or more extreme peaks and valleys relative to the average plane.

The 2D photo simulation below highlights the blue climbing grip’s surface morphology under artificial lighting.

2D photo simulation of the blue climbing grip surface showing pores, roughness, and morphology under artificial lighting.

Pore Morphology Analysis

A pore analysis was performed across the full scanned area using a semi-automated edge-detection algorithm. The analysis identified recessed surface features to quantify pore coverage, pore density, radius, void volume, and maximum depth.

Pore detection analysis of the blue climbing grip surface using semi-automated edge detection to identify recessed surface features.

The detected pore locations were mapped across the scanned 5 mm × 5 mm area to evaluate pore coverage, density, and size distribution.

Pore distribution map of the blue climbing grip sample showing detected recessed surface features across a 5 mm by 5 mm scanned area.
Information
Method Circle detection
Features detected Pores, recessed objects
Minimum detection diameter 0.040 mm
Maximum detection diameter 2.000 mm
Number of detected pores 794
Surface coverage 24.208%
Pore density 31.355 particles/mm²
Global Statistics
Parameter Unit Mean Std. Dev. Min Max
Radius mm 0.035 0.035 0.020 0.218
Void volume µm³ 821,872.849 2,495,310.021 11,009.819 2.929 × 10⁷
Maximum depth µm 476.053 305.830 16.132 1044.045

Pores covered 24.208% of the blue grip’s scanned surface, with a pore density of 31.355 particles/mm². The detected pores and cracks were highly heterogeneous in size, volume, and depth, ranging from large crater-like features with a maximum radius of 0.218 mm and void volume greater than 2.9 × 10⁷ µm³ to small pores with a minimum radius of 0.020 mm and void volume of approximately 1.1 × 10⁴ µm³.

This uneven distribution is reflected in the large standard deviation measured for void volume and maximum depth. The pore distribution is bimodal, with one population of fine, deep pores and another population of larger crater-like valleys.

Functional Surface Parameters (Abbott-Firestone curve)

The Abbott-Firestone curve shows the cumulative areal material distribution of the blue climbing grip sample. This analysis defines functional surface parameters including Sk, Spk, and Svk according to ISO 25178-2.

Abbott-Firestone curve for the blue climbing grip sample showing cumulative areal material distribution and functional surface parameters.
Information
Standard ISO 25178-2
Parameter Value Unit
Sk 522.359 µm
Spk 117.670 µm
Svk 295.209 µm
Smrk1 6.122 %
Smrk2 87.456 %

The chart below shows the peak-valley distribution from the mean plane based on the functional parameters derived from the Abbott-Firestone curve. Valleys are shown in purple, the mean plane in green, and peaks in orange.

Peak-valley distribution map of the blue climbing grip sample showing valleys, mean-plane regions, and peaks derived from Abbott-Firestone functional parameters.
Information
1st threshold Height – c1: 283.646 µm
2nd threshold Height – c2: -238.619 µm
Parameters Unit
Projected area (in %) % 12.544 81.334 6.122
Projected area mm² 3.182 20.629 1.553
Volume of material (in %) % 96.079 48.546 1.514
Volume of material µm³ 1.151 × 10¹⁰ 6.431 × 10⁹ 9.142 × 10⁷

The blue grip sample shows a dominant mean-plane region with fine, deep pores distributed across the surface and localized peak features. Compared with the yellow grip, the blue grip contains a higher projected peak area and a bimodal pore structure, combining fine recessed pores with larger crater-like valleys.

Schlussfolgerung

In this application, the NANOVEA JR25 Non-Contact Optical Profiler was used to measure the surface roughness, topography, and pore morphology of yellow and blue bouldering grip samples.

Topographic analysis showed that both grip samples had high surface roughness, with Sa values above 100 µm and Sz values above 1000 µm. Both surfaces also showed an asymmetric height distribution skewed toward valleys, indicating that recessed features played a major role in the measured surface morphology.

The yellow grip sample showed higher pore coverage, with pores covering 47.395% of the scanned surface. Its surface was mainly characterized by average-sized pores distributed across the measured area.

The blue grip sample showed lower pore coverage at 24.208%, but a much higher pore density of 31.355 particles/mm². Its pore distribution was bimodal, with a population of fine, deep pores and a separate population of larger crater-like valleys.

These results show how non-contact 3D optical profilometry can quantify climbing hold surface features that are difficult to evaluate from visual inspection alone, including roughness, pore coverage, pore depth, surface height distribution, and functional topography. The blue grip’s higher porosity and bimodal pore structure make it more likely to absorb moisture and chalk at the contact interface, while its elevated roughness and surface morphology support stable friction for shoe rubber and finger contact. The yellow grip’s lower roughness and flatter profile suggest it is better suited for use as a foothold in slab climbing, where broad surface contact matters more than deep textural engagement.

Frequently Asked Questions About Climbing Hold Surface Roughness

What is climbing hold surface roughness?

Climbing hold surface roughness describes the height variation, texture, pores, asperities, and valleys present on the surface of a climbing grip. These features can influence contact behavior between the hold, shoe rubber, skin, chalk, and moisture.

How can climbing hold surface roughness be measured?

Climbing hold surface roughness can be measured using non-contact 3D optical profilometry. This method reconstructs the surface topography and calculates areal roughness parameters such as Sa, Sz, Sp, Sv, Ssk, and Sku without touching or deforming the sample.

Why use non-contact optical profilometry for climbing hold analysis?

Non-contact optical profilometry is useful for climbing hold analysis because climbing grips can contain deep pores, sharp valleys, rough asperities, and irregular surface texture. A contact stylus may lose contact, fail to reach recessed features, or introduce artifacts on complex surfaces.

What does Sa mean in surface roughness analysis?

Sa is the arithmetic mean height of a surface and is commonly used to describe average areal surface roughness. In this app note, both climbing grip samples showed high Sa values above 100 µm, indicating strongly textured surfaces.

What does Sz mean in optical profilometry results?

Sz is the maximum height of the measured surface, calculated from the highest peak to the deepest valley. In climbing hold surface roughness analysis, Sz helps describe the full vertical range of the grip’s surface texture.

Why is pore morphology important for climbing grips?

Pore morphology can affect how a climbing grip interacts with chalk, sweat, humidity, skin, and shoe rubber. Measuring pore coverage, density, depth, and volume helps quantify surface features that are difficult to evaluate by visual inspection alone.

stent coating adhesion testing failure analysis drug eluting stent coating

Stent Coating Adhesion and Delamination Analysis Using Nano Scratch Testing

Application Note | Stent Coating Adhesion Testing

Stent Coating Adhesion and Delamination Analysis Using Nano Scratch Testing

Quantifying Coating Failure and Adhesion Performance on Drug-Eluting Stents

stent coating adhesion testing nano scratch delamination critical load

Research & Experimental Testing

Duanjie Li, PhD

Visual Design & Editorial

Andrew Shore

Einführung

Blood is carried through arteries from the heart to the rest of the body. Any weakening or blockage of these vessels can pose significant health risks and may become life-threatening. A stent is a small mesh tube inserted into the lumen of a blood vessel to treat narrowed or weakened arteries. Stent implantation is now a widely used procedure to support the arterial wall and restore blood flowᶦ.

Metal stent mesh geometry illustrating the structural complexity of vascular implant design.

Why coating adhesion matters in drug-eluting stents

Drug-eluting stents represent a major advancement in stent technology. They incorporate a biodegradable, biocompatible polymer coating that enables controlled drug release at the arterial site, helping to inhibit intimal thickening and reduce the risk of restenosisᶦᶦ.

A critical concern in these systems is the delamination of the polymer coating from the metallic stent substrate. This coating carries the drug-eluting layer, and its adhesion directly impacts device performance and reliability.

To improve coating adhesion, stents are often designed with complex geometries. In this study, the polymer coating is located at the bottom of grooves within the stent mesh. This configuration presents a significant challenge for adhesion measurement.

A reliable method is required to quantitatively evaluate the interfacial strength between the polymer coating and the metal substrate. The small diameter of the stent mesh, comparable to a human hair, combined with its three-dimensional geometry, requires:

  • ultrafine X-Y positioning accuracy
  • precise control of applied load
  • accurate depth measurement during testing

Measurement Method

Nano scratch testing is performed using the NANOVEA PB1000 Mechanischer Tester, in Nano Scratch Mode, to evaluate the cohesive and adhesive strength of the polymer coating on the metal mesh of stent samples.

Controlled scratch measurements are carried out on stent geometries with dimensions comparable to a human hair, enabling precise evaluation of coating adhesion on complex stent structures.

NANOVEA PB1000 Advanced

Mechanischer Tester

Testbedingungen

1. Regular Stent Samples

The stent is fixed on the sample stage, with a support wire inserted inside the stent tube to ensure stability during nano scratch testing. The NANOVEA Mechanical Tester is used to perform nano scratch measurements using the parameters summarized in Table 1, to evaluate the cohesive and adhesive strength of the polymer coating on the metal substrate.

ParameterValue
Load typeProgressiv
Initial load0.05 mN
Final load300 and 100 mN
Sliding speed0.5 mm/min
Sliding distance0.5 mm
Indenter geometryKonisch
Indenter material (tip)Diamant
Radius der Eindringkörperspitze20 µm
Temperatur24°C (room)

Tabelle 1: Test parameters for nano scratch measurements on regular stent samples

2. Grooved Stent Samples

The SEM image in Fig. 1 shows the cross-section of the stent sample. The stent features a groove with a depth of approximately 30 µm. The polymer coating, with a thickness of 10.8 µm, is located at the bottom of the groove.

Standard 60° conical diamond tips are not sharp enough to reach the bottom of the groove without contacting the sidewalls. Therefore, a sharper 40° conical diamond tip is used in this study (Fig. 2).

Nano scratch measurements are performed using the parameters summarized in Table 2.

Parameter Value
Load type Progressiv
Initial load 0.1 mN
Final load 300 mN
Ladegeschwindigkeit 300 mN/min
Scratch length 0.25 mm
Scratch speed 0.25 mm/min
Indenter geometry 40° cone
Indenter material (tip) Diamant
Radius der Eindringkörperspitze 5 µm

Table 2: Test parameters for nano scratch measurements on grooved stent samples

stent groove cross section polymer coating thickness adhesion analysis nano scratch testing

Fig. 1: SEM cross-section of a grooved stent showing polymer coating located at the bottom of the groove, highlighting the challenge of coating adhesion measurement in recessed geometries.

nano scratch diamond tip 40 degree stent groove coating adhesion testing schematic

Fig. 2: Schematic of a 40° conical diamond tip designed for nano scratch testing inside stent grooves, enabling accurate adhesion measurement without sidewall interference.

Ergebnisse und Diskussion

The stent mesh has a diameter of approximately 100 μm, comparable to a human hair. Precise positioning is therefore critical to ensure the scratch test is performed at the center of the stent mesh. The NANOVEA Mechanical Tester provides X–Y positioning accuracy down to 0.25 μm, enabling accurate test placement under the integrated optical microscope.

1. Regular Stent Samples

Nano scratch testing is performed with a progressively increasing load up to 300 mN. The full scratch track on the stent is shown in Fig. 3a, while failure behavior at different stages is presented in Fig. 3b and 3c.

Two critical loads are identified:

  • Lc1: the load at which the first visible damage appears on the coating
  • Lc2: the load at which the coating is fully removed and the substrate is exposed

The evolution of coefficient of friction (COF) and penetration depth is shown in Fig. 4, providing insight into the progression of coating failure during the test.

The first signs of coating damage appear at Lc1 ≈ 14.5 mN. As the applied load increases, the diamond tip progressively penetrates the polymer coating, resulting in a wider and deeper scratch track. During this phase, the COF increases from approximately 0.05 to 0.7.

At Lc2 ≈ 78.1 mN, the coating is fully delaminated from the metal substrate. Beyond this point, as the load continues to increase, both COF and penetration depth remain relatively stable due to the mechanical support of the underlying metal substrate.

nano scratch track stent coating progressive load adhesion testing

(a) Full Scratch Track

(b) Lc1 ≈ 14.5 mN

stent coating delamination lc2 nano scratch 78.1 mN adhesion testing

(c) Lc2 ≈ 78.1 mN

Fig. 3: Nano scratch track on a stent coating under progressively increasing load, showing (a) full scratch path, (b) initial coating failure at Lc1 ≈ 14.5 mN, and (c) complete coating delamination at Lc2 ≈ 78.1 mN.

nano scratch testing stent coating coefficient of friction depth progression adhesion failure

Fig. 4: Evolution of coefficient of friction (COF) and penetration depth during nano scratch testing of a stent coating under progressively increasing load, showing the progression of coating failure and transition to substrate support.

Failures during nano scratch testing up to a maximum load of 300 mN occur at critical loads below 100 mN. To enable a more quantitative comparison of coating performance, additional tests are performed with a maximum load of 100 mN on two stent samples, referred to as Sample 1 and Sample 2.

Fig. 5 compares the scratch tracks of Sample 1 and Sample 2 after nano scratch testing. Sample 1 exhibits the first sign of coating damage at a critical load of Lc1 ≈ 13.2 mN, while Sample 2 shows initial failure at a higher load of Lc1 ≈ 21.1 mN.

Coating delamination occurs at 62.5 mN for Sample 1. In contrast, the coating on Sample 2 remains intact throughout the test, continuing to protect the metal substrate under the same loading conditions.

This behavior is further reflected in the evolution of coefficient of friction (COF) and penetration depth, as shown in Fig. 6. When the diamond tip penetrates through the coating and contacts the metal substrate in Sample 1, the COF reaches a peak while the penetration depth decreases due to the increased stiffness of the underlying substrate.

stent coating sample 1 early failure nano scratch track delamination adhesion testing

(a) Sample 1 – Early Coating Failure

stent coating sample 2 high adhesion nano scratch track minimal damage testing

(b) Sample 2 – Improved Coating Integrity

Fig. 5: Comparison of nano scratch tracks for two stent coatings, showing (a) early coating failure and delamination in Sample 1, and (b) improved coating integrity in Sample 2 under the same loading conditions.

nano scratch testing stent coating COF depth comparison sample 1 sample 2 adhesion performance

Fig. 6: Comparison of coefficient of friction (COF) and penetration depth for Sample 1 and Sample 2 during nano scratch testing, showing earlier substrate contact and higher friction response in Sample 1, indicating weaker coating adhesion.

2. Grooved Stent Samples

As shown in Fig. 1 and Fig. 7, the grooved stent mesh has a diameter of approximately 90 μm, comparable to a human hair. The groove has a width of ~50 μm and a depth of 30 μm. This geometry presents a significant challenge for nano scratch testing, particularly for evaluating coating adhesion at the bottom of the groove.

Precise positioning is critical to locate the scratch test within the groove. The nano scratch test is performed with a progressively increasing load up to 300 mN. The full scratch tracks of grooved stent Samples 3 and 4 are compared in Fig. 7.

The critical load Lc is defined as the load at which the coating fails and the substrate becomes exposed. The evolution of normal load and penetration depth, shown in Fig. 8, provides further insight into the progression of coating failure during testing.

As the applied load increases, the diamond tip progressively penetrates the polymer coating, resulting in a deeper scratch track. When the critical load Lc is reached, the coating delaminates from the metal substrate.

Sample 3 exhibits coating failure at Lc ≈ 126 mN, while Sample 4 fails at a higher load of Lc ≈ 173 mN. This difference indicates stronger adhesion of the coating in Sample 4.

The measured critical loads enable quantitative comparison of coating adhesion performance. Under the same testing conditions, the coating on Sample 4 demonstrates higher resistance to delamination, making it the better-performing candidate in this study.

stent groove coating failure sample 3 nano scratch 126 mN adhesion testing

(c) Sample 3 – Coating Failure in Groove (Lc ≈ 126 mN)

stent groove coating adhesion sample 4 nano scratch 173 mN minimal failure testing

(d) Sample 4 – Higher Adhesion in Groove (Lc ≈ 173 mN)

Fig. 7: Nano scratch tracks inside stent grooves for Samples 3 and 4, showing (c) coating failure at Lc ≈ 126 mN in Sample 3 and (d) higher adhesion with delayed failure at Lc ≈ 173 mN in Sample 4.

(a) Sample 3 – Earlier Coating Failure (Lc ≈ 126 mN)

(b) Sample 4 – Delayed Failure and Higher Adhesion (Lc ≈ 173 mN)

Fig. 8: Evolution of normal load and penetration depth during nano scratch testing inside stent grooves for Samples 3 and 4, showing earlier coating failure in Sample 3 and delayed failure at higher load in Sample 4. The vertical green line indicates the critical load (Lc) where coating delamination occurs.

Schlussfolgerung

This study demonstrates the ability of the NANOVEA Mechanical Tester to quantitatively evaluate the cohesive and adhesive strength of polymer coatings on both regular and grooved stent geometries using nano scratch testing.

The recessed geometry of the stent grooves, approximately 50 μm wide and 30 μm deep, presents a significant challenge for coating adhesion measurement. The high X–Y positioning accuracy of 0.25 μm enables precise placement of the scratch test within these confined regions, allowing direct evaluation of coating performance where failure is most critical.

By applying a controlled, progressively increasing load, critical loads associated with coating failure can be identified and compared across samples. This approach enables reliable differentiation of coating adhesion performance and interfacial integrity, even on small, complex stent structures.

Referenzen

[I] http://www.nhlbi.nih.gov/health/health-topics/topics/stents
[II] http://www.scielo.org.mx/scielo.php?script=sci_arttext&pid=S1405-99402006000300008

Frequently Asked Questions About Stent Coating Adhesion Testing

What is stent coating adhesion testing?

Stent coating adhesion testing evaluates how strongly a polymer coating is bonded to the metal substrate of a stent. Techniques such as nano scratch testing quantify the load at which coating damage and delamination occur, providing measurable indicators of adhesion strength.

What is critical load (Lc) in nano scratch testing?

Critical load (Lc) is the applied load at which a coating fails during a scratch test.

  • Lc1 corresponds to the first visible damage in the coating
  • Lc2 indicates complete coating removal and exposure of the substrate

These values are used to quantify and compare coating adhesion performance.

Why is coating adhesion important in drug-eluting stents?

Coating adhesion directly affects the reliability of drug-eluting stents. Poor adhesion can lead to coating delamination, which may compromise controlled drug release and increase the risk of device failure.

How do you measure coating adhesion inside stent grooves?

Measuring adhesion inside stent grooves requires high positioning accuracy and appropriate indenter geometry. Nano scratch testing with sharp diamond tips allows access to recessed coating regions, enabling direct evaluation of adhesion within complex stent geometries.

What does coefficient of friction (COF) indicate in scratch testing?

The coefficient of friction (COF) reflects changes in surface interaction during the scratch test. A sudden increase in COF often indicates coating failure and contact between the indenter and the underlying metal substrate.

How can nano scratch testing compare different coating formulations?

Nano scratch testing enables direct comparison of coatings by measuring critical loads under controlled conditions. Higher critical loads indicate stronger adhesion and improved resistance to delamination, allowing selection of better-performing coating systems.

Dentist holding dental model for tooth surface roughness analysis and 3D reconstruction

Dental Surface Roughness Measurement & 3D Tooth Topography

Application Note | Dental Surface Characterization

Dental Surface Roughness Measurement and Full 3D Tooth Topography

Surface Roughness Analysis Using Non-Contact Optical Profilometry

Dental surface roughness measurement and 3D molar reconstruction using optical profilometry

Vorbereitet von

Walter Alabiso, PhD; Davide Morrone, MPhys; Andrew Shore, MA

Einführung

The ability to accurately characterize tooth surfaces, including micro-roughness and 3D surface topography at the nanometer scale, enables advanced research and applications in orthodontics and dental materials science. Non-contact optical profilometry provides a precise method for measuring dental surface roughness and analyzing tooth surface morphology without damaging delicate structures. These measurements support the development of composite dental materials that replicate the natural surface roughness of enamel, as well as the design and fabrication of patient-specific dental casts and restorative components.

Low surface roughness plays a primary role in limiting bacterial adhesion and plaque formation, thereby reducing the risk of cavities. An increase in average roughness (Ra) above 2 µm leads to a steep increase in biofilm formation in vivo.¹ An Ra of 0.2 µm is considered the threshold value below which no further reduction in bacterial adhesion can be expected.²

Reconstruction of the tooth’s 3D surface topography enables the fabrication of dental casts, which are essential for accurate diagnosis, treatment planning, and the fabrication of dental appliances.

Non-Contact Optical Profilometry for Dental Surface Analysis

The present study illustrates the potential of NANOVEA’s high-precision non-contact optical profilometers for dental surface roughness measurement and 3D tooth topography analysis. Chromatic Light technology offers significant advantages over classical touch probe techniques. It acquires data points from deep crevices and complex geometries without introducing measurement errors or artifacts caused by local plastic deformation and without requiring extensive data manipulation.

Compared to focus variation systems, single-point optical sensing provides superior lateral and height accuracy, with X/Y resolution below 0.5 µm, maximum vertical resolution of 1.9 nm, and the ability to measure surface angles up to 87°. The technique is effective on transparent, opaque, specular, diffusive, polished, and rough dental surfaces, making it well suited for comprehensive dental surface characterization.

Measurement Method

Bei dieser Anwendung ist die NANOVEA JR25 Non-Contact Optical Profiler was used to analyze the surface roughness and 3D surface topography of an adult human molar previously affected by tooth decay. The side of the tooth was scanned using a PS2–MG140 single-point optical sensor to measure surface roughness parameters over a defined region of interest and along multiple line profiles.

The crown of the tooth was then scanned and reconstructed using a PS5–MG35 single-point optical sensor, which is suited for larger-area acquisition and full 3D tooth topography measurement.


NANOVEA JR25 Portable
Optisches Profilometer

Surface Measurement Using NANOVEA Optical Profilometer

Surface roughness measurements were performed on the lateral side of the molar crown, followed by full 3D reconstruction of the crown surface. Separate single-point optical sensors were used to optimize measurement accuracy for both localized roughness analysis and large-area surface topography acquisition.

PS2 – MG140

Surface roughness analysis by area and parallel line profiles on the side of the tooth’s crown.

PS5 – MG35

Full 3D surface reconstruction of the tooth’s crown.

Messparameter

The following measurement parameters were used for localized surface roughness analysis and full 3D surface reconstruction of the molar crown using NANOVEA single-point optical sensors.

ParameterRoughness Analysis (Area)Roughness Analysis (Profiles)Full 3D Reconstruction
Optical PenPS2-MG140PS2-MG140PS5-MG35
Z-Range [µm]30030010000
X-Distance [mm]2.003.007.50
X-Step Size [µm]1.701.7010.00
Y-Distance [mm]2.001.007.00
Y-Step Size [µm]1.70100.0010.00
Averaging (Avg)111
Measurement TypeDirectDirectDirect
Acquisition ModeSingle FrequencySingle FrequencyDual Frequency
Acquisition Rate [Hz]200200100–400
Light Intensity [%]100100100

Optical Profilometry Results

Surface Roughness Analysis (AREA)

 The single-point optical sensor PS2 was used to investigate fine features of the tooth’s side surface. The following picture represents a false-color 2D map of the scanned region:

False-color 2D height map of scanned tooth surface region

A least-squares degree-8 polynomial form removal was applied to isolate the surface roughness component. The roughness filters S-Gaussian 2.5 µm and L-Gaussian 0.8 mm were then applied according to ISO 25178. The resulting filtered surface and corresponding roughness parameters are presented below.

ISO 25178 – Roughness (S-L)
S-filter (λs): Gaussian, 2.5 µm
F: [Workflow] Form removed (LS-poly 8)
L-filter (λc): Gaussian, 0.8 mm
Height Parameters
Sq2.433µmWurzel-Mittel-Quadrat-Höhe
Ssk-0.102 Schrägheit
Sku3.715 Kurtosis
Sp18.861µmMaximale Peakhöhe
Sv16.553µmMaximum pit depth
Sz35.414µmMaximale Höhe
Sa1.888µmArithmetisches Mittel der Höhe

The average surface roughness Sa is 1.888 µm, while the peak-to-valley height Sz reaches 35.414 µm.

A 3D surface rendering of the filtered area is shown below for visualization.

3D rendering of ISO 25178 filtered tooth surface roughness

Roughness Analysis (Profiles)

Surface roughness profiles were measured using a series of 11 parallel line scans along the X direction on the side of the tooth. The false-color 2D surface map of the raw scan is shown below.

False-color 2D raw scan of tooth surface for line roughness profiles

The surface form was removed using a least-squares 8-degree polynomial prior to applying the metrological filters, leaving the residual surface shown below.

A statistical analysis of the measured surface roughness profiles reveals the following line roughness parameters.

Overlay of multiple tooth surface roughness profiles for statistical analysis

ISO 4287 – Roughness (S-L)
F: Keiner
S-filter (λs): Gaussian, 2.5 µm
L-filter (λc): Gaussian, 0.8 mm
Evaluation length: All λc (3)
Amplitude Parameters – Roughness Profile
  DescriptionMeanStd devMinMax
RpµmMaximum peak height of the roughness profile5.6830.7614.3156.610
RvµmMaximum valley depth of the roughness profile6.2421.0094.7018.438
RzµmMaximum height of roughness profile11.9251.6769.12315.048
RaµmArithmetic mean deviation of the roughness profile2.0630.2971.7102.629
RqµmRoot-mean-square (RMS) deviation of the roughness profile2.5230.3612.0573.175

ISO 4287 – Roughness (S-L)
F: Keiner
S-filter (λs): Gaussian, 2.5 µm
L-filter (λc): Gaussian, 0.8 mm
Evaluation length: All λc (3)
Amplitude Parameters – Roughness Profile
Rpµm
Maximum peak height of the roughness profile
Mean5.683
Std dev0.761
Min4.315
Max6.610
Rvµm
Maximum valley depth of the roughness profile
Mean6.242
Std dev1.009
Min4.701
Max8.438
Rzµm
Maximum height of roughness profile
Mean11.925
Std dev1.676
Min9.123
Max15.048
Raµm
Arithmetic mean deviation of the roughness profile
Mean2.063
Std dev0.297
Min1.710
Max2.629
Rqµm
Root-mean-square (RMS) deviation of the roughness profile
Mean2.523
Std dev0.361
Min2.057
Max3.175

The value of Ra is consistent with the Sa value extracted from the surface area measurement.

Different metrological filters can be applied to distinguish between macroscopic waviness and microscopic surface roughness. For example, a coarser filter cut-off, such as the 8 mm cut-off used with the Robust Gaussian order-2 filter, produces a smoother waviness profile (red) that is less sensitive to sharp local variations and follows the original surface profile more loosely.

Comparison of waviness and roughness profiles on tooth surface using coarse filter

Alternatively, a finer cut-off (e.g., 0.08 mm) enables the analysis of micro-roughness by removing the waviness component that follows the original profile at a larger scale, leaving the finer surface roughness features of the tooth visible.

The microroughness analysis obtained using a 0.08 mm L-Gaussian filter is presented below.

Final microroughness profile of tooth surface after filtering

ISO 4287 – Roughness (S-L)
F: Keiner
S-filter (λs): Gaussian, 2.5 µm
L-filter (λc): Gaussian, 0.08 mm
Evaluation length: All λc (37)
Amplitude Parameters – Roughness Profile
  DescriptionMeanStd devMinMax
RpµmMaximum peak height of the roughness profile1.5820.1221.3421.748
RvµmMaximum valley depth of the roughness profile1.4660.1191.2541.661
RzµmMaximum height of roughness profile3.0490.1962.8203.409
RaµmArithmetic mean deviation of the roughness profile0.4950.0470.4230.597
RqµmRoot-mean-square (RMS) deviation of the roughness profile0.6430.0560.5620.762

ISO 4287 – Roughness (S-L)
F: Keiner
S-filter (λs): Gaussian, 2.5 µm
L-filter (λc): Gaussian, 0.8 mm
Evaluation length: All λc (3)
Amplitude Parameters – Roughness Profile
Rpµm
Maximum peak height of the roughness profile
Mean5.683
Std dev0.761
Min4.315
Max6.610
Rvµm
Maximum valley depth of the roughness profile
Mean6.242
Std dev1.009
Min4.701
Max8.438
Rzµm
Maximum height of roughness profile
Mean11.925
Std dev1.676
Min9.123
Max15.048
Raµm
Arithmetic mean deviation of the roughness profile
Mean2.063
Std dev0.297
Min1.710
Max2.629
Rqµm
Root-mean-square (RMS) deviation of the roughness profile
Mean2.523
Std dev0.361
Min2.057
Max3.175

Full 3D Tooth Surface Topography Reconstruction

The extended Z-scan range of the PS5 optical sensor enables high-fidelity scanning of the entire tooth crown surface. The resulting 3D surface topography is shown below.

False-color surface topography map of full tooth crown measured with optical profilometer

2D VIEW: 2D surface map of the tooth crown measured with optical profilometry

3D surface reconstruction of molar crown from optical profilometer scan

3D VIEW: High-fidelity 3D rendering of the molar crown surface obtained with optical profilometry

Schlussfolgerung

In this application, the NANOVEA JR25 Non-Contact Optical Profiler was used to measure the surface roughness and 3D surface topography of an adult human molar.

Both the area scan and the line profile analysis revealed a roughness Rq of approximately 2.5 µm and an Ra of about 1.9–2.0 µm. These values are consistent with results reported in the literature.³ The use of a narrower L-Gaussian filter with an 80 µm cut-off enabled further investigation of micro-roughness, revealing an Rq of 0.643 µm and an Ra of 0.495 µm.

The full 3D surface topography of the molar crown was reconstructed with high fidelity. The high measurement resolution allows detection of fine surface features and crevices. The resulting surface data can be easily processed and exported as STL files, enabling the design and fabrication of customized dental devices and restorative components.

Referenzen

[1] Shin, B.W., et al. Surface Roughness of Prefabricated Pediatric Zirconia Crowns Following Simulated Toothbrushing. Pediatric Dentistry 44.5 (2022): 363–367.
[2] Bollen, C.M.L., Paul Lambrechts, and Marc Quirynen. Comparison of surface roughness of oral hard materials to the threshold surface roughness for bacterial plaque retention: A review of the literature. Dental Materials 13.4 (1997): 258–269.
[3] Suputtamongkol, K., et al. Surface roughness resulting from wear of lithia-disilicate-based posterior crowns. Wear 269.3–4 (2010): 317–322.

Frequently Asked Questions About Dental Surface Roughness Measurement

What is dental surface roughness measurement?

Dental surface roughness measurement quantifies the microscopic texture of tooth surfaces using parameters such as Ra, Rq, and Sa. Optical profilometers measure these features without contacting the surface, allowing accurate analysis of enamel, restorative materials, and dental crowns.

Why use optical profilometry to measure tooth roughness?

Optical profilometry provides non-contact surface measurement with nanometer-scale vertical resolution. It captures 2D surface maps and full 3D surface topography of dental structures without damaging soft or polished surfaces.

What roughness parameters are used for dental surface analysis?

Common roughness parameters include Ra (arithmetic mean roughness), Rq (root mean square roughness), Sa (areal roughness), and Sz (maximum surface height). These parameters help evaluate enamel wear, plaque adhesion risk, and the performance of restorative materials.

Why is surface roughness important in dentistry?

Surface roughness affects plaque retention, wear resistance, and the long-term performance of dental restorations. Controlling micro-roughness can reduce bacterial adhesion and improve the durability of dental materials.

Need Reliable Surface Roughness Measurement for Dental Materials?

Analyse kugelgestrahlter Oberflächen

ANALYSE DER KUGELGESTRAHLTEN OBERFLÄCHE

VERWENDUNG DES BERÜHRUNGSLOSEN 3D-PROFILOMETERS

Vorbereitet von

CRAIG LEISING

EINFÜHRUNG

Beim Kugelstrahlen handelt es sich um einen Prozess, bei dem ein Substrat mit kugelförmigen Metall-, Glas- oder Keramikperlen – allgemein als „Schuss“ bezeichnet – mit einer Kraft bombardiert wird, die darauf abzielt, der Oberfläche Plastizität zu verleihen. Die Analyse der Eigenschaften vor und nach dem Strahlen liefert entscheidende Erkenntnisse zur Verbesserung des Prozessverständnisses und der Prozesskontrolle. Besonders hervorzuheben sind die Oberflächenrauheit und die Abdeckungsfläche der durch den Schuss hinterlassenen Grübchen.

Bedeutung des berührungslosen 3D-Profilometers für die Analyse kugelgestrahlter Oberflächen

Im Gegensatz zu herkömmlichen Kontaktprofilometern, die traditionell für die Analyse von kugelgestrahlten Oberflächen verwendet werden, liefert die berührungslose 3D-Messung ein vollständiges 3D-Bild, um ein umfassenderes Verständnis des Erfassungsbereichs und der Oberflächentopographie zu ermöglichen. Ohne 3D-Funktionen stützt sich eine Inspektion ausschließlich auf 2D-Informationen, die zur Charakterisierung einer Oberfläche nicht ausreichen. Das Verständnis der Topographie, des Abdeckungsbereichs und der Rauheit in 3D ist der beste Ansatz zur Steuerung oder Verbesserung des Strahlprozesses. NANOVEAs Berührungslose 3D-Profilometer Nutzen Sie die Chromatic Light-Technologie mit der einzigartigen Fähigkeit, steile Winkel auf bearbeiteten und gestrahlten Oberflächen zu messen. Wenn andere Techniken aufgrund von Sondenkontakt, Oberflächenschwankungen, Winkel oder Reflexionsvermögen keine zuverlässigen Daten liefern, sind NANOVEA-Profilometer außerdem erfolgreich.

MESSZIEL

In dieser Anwendung wird das berührungslose Profilometer NANOVEA ST400 zur Messung von Rohmaterial und zwei unterschiedlich gestrahlten Oberflächen für eine vergleichende Überprüfung verwendet. Es gibt eine endlose Liste von Oberflächenparametern, die nach dem 3D-Oberflächenscan automatisch berechnet werden können. Hier überprüfen wir die 3D-Oberfläche und wählen Bereiche von Interesse für die weitere Analyse aus, einschließlich der Quantifizierung und Untersuchung der Rauheit, Grübchen und Oberfläche.

NANOVEA ST400 Standard
Optisches 3D-Profilometer

DIE PROBE

Prüfung der kugelgestrahlten Oberfläche

ERGEBNISSE

STAHLOBERFLÄCHE

Kugelgestrahlte Oberflächenrauheit
Charakterisierung von kugelgestrahlten Oberflächen

ISO 25178 3D-RAUHEITSPARAMETER

SA 0,399 μm Durchschnittliche Rauheit
Sq 0,516 μm RMS-Rauheit
Sz 5,686 μm Maximaler Abstand vom Gipfel zum Tal
Sp 2,976 μm Maximale Spitzenhöhe
Sv 2,711 μm Maximale Grubentiefe
Sku 3.9344 Kurtosis
Ssk -0.0113 Schrägheit
Sal 0,0028 mm Autokorrelationslänge
Str 0.0613 Textur-Seitenverhältnis
Sdar 26,539 mm² Oberfläche
Svk 0,589 μm Reduzierte Taltiefe
 

ERGEBNISSE

GESTRAHLTE OBERFLÄCHE 1

Kugelgestrahltes Oberflächenprofil
Kugelgestrahltes Oberflächenprofilometer

OBERFLÄCHENABDECKUNG 98.105%

Untersuchung der kugelgestrahlten Oberfläche

ISO 25178 3D-RAUHEITSPARAMETER

Sa 4,102 μm Durchschnittliche Rauheit
Sq 5,153 μm RMS-Rauheit
Sz 44,975 μm Maximaler Abstand vom Gipfel zum Tal
Sp 24,332 μm Maximale Spitzenhöhe
Sv 20,644 μm Maximale Grubentiefe
Sku 3.0187 Kurtosis
Ssk 0.0625 Schrägheit
Sal 0,0976 mm Autokorrelationslänge
Str 0.9278 Textur-Seitenverhältnis
Sdar 29,451 mm² Oberfläche
Svk 5,008 μm Reduzierte Taltiefe

ERGEBNISSE

GESTRAHLTE OBERFLÄCHE 2

Kugelgestrahlte Oberflächenprüfung
Analyse einer kugelgestrahlten Oberfläche

OBERFLÄCHENABDECKUNG 97.366%

Oberflächenmesstechnik für kugelgestrahlte Oberflächen

ISO 25178 3D-RAUHEITSPARAMETER

Sa 4.330 μm Durchschnittliche Rauheit
Sq 5,455 μm RMS-Rauheit
Sz 54,013 μm Maximaler Abstand vom Gipfel zum Tal
Sp 25,908 μm Maximale Spitzenhöhe
Sv 28,105 μm Maximale Grubentiefe
Sku 3.0642 Kurtosis
Ssk 0.1108 Schrägheit
Sal 0,1034 mm Autokorrelationslänge
Str 0.9733 Textur-Seitenverhältnis
Sdar 29,623 mm² Oberfläche
Svk 5,167 μm Reduzierte Taltiefe

SCHLUSSFOLGERUNG

In dieser Anwendung zur kugelgestrahlten Oberflächenanalyse haben wir gezeigt, wie der NANOVEA ST400 3D Non-Contact Profiler sowohl die Topographie als auch die Nanometerdetails einer gestrahlten Oberfläche präzise charakterisiert. Es ist offensichtlich, dass sowohl Oberfläche 1 als auch Oberfläche 2 im Vergleich zum Rohmaterial einen erheblichen Einfluss auf alle hier angegebenen Parameter haben. Eine einfache visuelle Betrachtung der Bilder offenbart die Unterschiede zwischen den Oberflächen. Dies wird durch die Beobachtung des Abdeckungsbereichs und der aufgeführten Parameter weiter bestätigt. Im Vergleich zu Oberfläche 2 weist Oberfläche 1 eine geringere durchschnittliche Rauheit (Sa), flachere Dellen (Sv) und eine geringere Oberfläche (Sdar) auf, aber eine etwas größere Abdeckungsfläche.

Anhand dieser 3D-Oberflächenmessungen können interessierende Bereiche leicht identifiziert und einer umfassenden Reihe von Messungen unterzogen werden, darunter Rauheit, Oberflächenbeschaffenheit, Textur, Form, Topographie, Ebenheit, Verzug, Ebenheit, Volumen, Stufenhöhe und andere. Für eine detaillierte Analyse kann schnell ein 2D-Querschnitt ausgewählt werden. Diese Informationen ermöglichen eine umfassende Untersuchung gestrahlter Oberflächen unter Nutzung einer vollständigen Palette von Oberflächenmessressourcen. Spezifische Interessengebiete könnten mit einem integrierten AFM-Modul weiter untersucht werden. NANOVEA 3D-Profilometer bieten Geschwindigkeiten von bis zu 200 mm/s. Sie können in Bezug auf Größe, Geschwindigkeit und Scanfunktionen individuell angepasst werden und erfüllen sogar die Reinraumstandards der Klasse 1. Optionen wie Indexierförderer und Integration für Inline- oder Online-Nutzung sind ebenfalls verfügbar.

Ein besonderer Dank gilt Herrn Hayden vom IWF für die Bereitstellung des in diesem Vermerk gezeigten Musters. Industrial Metal Finishing Inc. | indmetfin.com

Morphologie der Lackoberfläche

MORPHOLOGIE DER LACKOBERFLÄCHE

AUTOMATISCHE ÜBERWACHUNG DER ENTWICKLUNG IN ECHTZEIT
MIT NANOVEA 3D PROFILOMETER

Morphologie der Lackoberfläche

Vorbereitet von

DUANJIE LI, PhD

EINFÜHRUNG

Die schützenden und dekorativen Eigenschaften von Lacken spielen in einer Vielzahl von Branchen eine wichtige Rolle, z. B. in der Automobil-, Marine-, Militär- und Bauindustrie. Um die gewünschten Eigenschaften wie Korrosionsbeständigkeit, UV-Schutz und Abriebfestigkeit zu erreichen, werden Lackrezepturen und -strukturen sorgfältig analysiert, modifiziert und optimiert.

BEDEUTUNG DES BERÜHRUNGSLOSEN 3D-PROFILOMETERS FÜR DIE ANALYSE DER OBERFLÄCHENMORPHOLOGIE TROCKNENDER FARBEN

Farbe wird in der Regel in flüssiger Form aufgetragen und durchläuft einen Trocknungsprozess, bei dem die Lösungsmittel verdampfen und sich die flüssige Farbe in einen festen Film verwandelt. Während des Trocknungsprozesses verändert die Lackoberfläche allmählich ihre Form und Textur. Durch die Verwendung von Additiven, die die Oberflächenspannung und die Fließeigenschaften des Lacks verändern, können verschiedene Oberflächenbeschaffenheiten und Texturen entwickelt werden. Im Falle einer schlecht formulierten Lackrezeptur oder einer unsachgemäßen Oberflächenbehandlung kann es jedoch zu unerwünschten Lackoberflächenfehlern kommen.

Eine genaue In-situ-Überwachung der Farboberflächenmorphologie während der Trocknungsperiode kann direkte Einblicke in den Trocknungsmechanismus liefern. Darüber hinaus ist die Echtzeitentwicklung von Oberflächenmorphologien eine sehr nützliche Information für verschiedene Anwendungen, beispielsweise beim 3D-Druck. Die NANOVEA Berührungslose 3D-Profilometer Messen Sie die Farboberflächenmorphologie von Materialien, ohne die Probe zu berühren, und vermeiden Sie Formveränderungen, die durch Kontakttechnologien wie einen gleitenden Stift verursacht werden können.

MESSZIEL

In dieser Anwendung wird das berührungslose Profilometer NANOVEA ST500, das mit einem optischen Hochgeschwindigkeits-Zeilensensor ausgestattet ist, zur Überwachung der Morphologie der Lackoberfläche während der einstündigen Trocknungszeit eingesetzt. Wir zeigen die Fähigkeit des berührungslosen Profilometers NANOVEA zur automatisierten Echtzeit-3D-Profilmessung von Materialien mit kontinuierlicher Formveränderung.

NANOVEA ST500 Großfläche
Optisches 3D-Profilometer

ERGEBNISSE & DISKUSSION

Die Farbe wurde auf die Oberfläche eines Metallblechs aufgetragen, woraufhin sofort automatische Messungen der Morphologieentwicklung der trocknenden Farbe in situ mit dem berührungslosen Profilometer NANOVEA ST500 durchgeführt wurden, das mit einem Hochgeschwindigkeits-Zeilensensor ausgestattet ist. Ein Makro wurde programmiert, um die 3D-Oberflächenmorphologie in bestimmten Zeitintervallen automatisch zu messen und aufzuzeichnen: 0, 5, 10, 20, 30, 40, 50 und 60 Minuten. Dieses automatisierte Scanverfahren ermöglicht es den Benutzern, Scanaufgaben automatisch auszuführen, indem sie festgelegte Verfahren nacheinander ablaufen lassen, was den Aufwand, die Zeit und mögliche Benutzerfehler im Vergleich zu manuellen Tests oder wiederholten Scans erheblich reduziert. Diese Automatisierung erweist sich als äußerst nützlich für Langzeitmessungen, bei denen mehrere Scans in unterschiedlichen Zeitabständen durchgeführt werden.

Der optische Zeilensensor erzeugt eine helle Linie, die aus 192 Punkten besteht, wie in ABBILDUNG 1 dargestellt. Diese 192 Lichtpunkte tasten die Probenoberfläche gleichzeitig ab, was die Scangeschwindigkeit erheblich erhöht. Dadurch wird sichergestellt, dass jeder 3D-Scan schnell abgeschlossen wird, um wesentliche Oberflächenveränderungen während jedes einzelnen Scans zu vermeiden.

Lackbeschichtungsanalyse mit 3D-Profilometer

ABBILDUNG 1: Optischer Zeilensensor, der die Oberfläche der trocknenden Farbe abtastet.

Die Falschfarbenansicht, die 3D-Ansicht und das 2D-Profil der Topografie der trocknenden Farbe zu repräsentativen Zeitpunkten sind in ABBILDUNG 2, ABBILDUNG 3 bzw. ABBILDUNG 4 dargestellt. Die Falschfarben in den Bildern erleichtern die Erkennung von Merkmalen, die nicht ohne weiteres zu erkennen sind. Unterschiedliche Farben stehen für Höhenunterschiede in verschiedenen Bereichen der Probenoberfläche. Die 3D-Ansicht ist ein ideales Hilfsmittel für den Benutzer, um die Lackoberfläche aus verschiedenen Blickwinkeln zu betrachten. Während der ersten 30 Minuten des Tests wechseln die Falschfarben auf der Lackoberfläche allmählich von wärmeren zu kühleren Tönen, was auf eine fortschreitende Abnahme der Höhe in diesem Zeitraum hindeutet. Dieser Prozess verlangsamt sich, wie die leichte Farbveränderung beim Vergleich des Lacks nach 30 und 60 Minuten zeigt.

Die durchschnittliche Probenhöhe und die Rauheit Sa in Abhängigkeit von der Trocknungszeit des Lacks sind in ABBILDUNG 5 dargestellt. Die vollständige Rauheitsanalyse des Lacks nach 0, 30 und 60 Minuten Trocknungszeit ist in TABELLE 1 aufgeführt. Es ist zu beobachten, dass die durchschnittliche Höhe der Lackoberfläche in den ersten 30 Minuten der Trocknungszeit rasch von 471 auf 329 µm abnimmt. Die Oberflächentextur entwickelt sich gleichzeitig mit dem Verdampfen des Lösungsmittels, was zu einem Anstieg des Rauhigkeitswertes Sa von 7,19 auf 22,6 µm führt. Danach verlangsamt sich der Lacktrocknungsprozess, was zu einer allmählichen Abnahme der Probenhöhe und des Sa-Wertes auf 317 µm bzw. 19,6 µm nach 60 Minuten führt.

Diese Studie unterstreicht die Fähigkeiten des berührungslosen NANOVEA 3D-Profilometers bei der Überwachung der 3D-Oberflächenveränderungen der trocknenden Farbe in Echtzeit, was wertvolle Einblicke in den Trocknungsprozess der Farbe ermöglicht. Durch die Messung der Oberflächenmorphologie ohne Berührung der Probe vermeidet das Profilometer Formveränderungen der ungetrockneten Farbe, wie sie bei Kontakttechnologien wie dem gleitenden Taststift auftreten können. Dieser berührungslose Ansatz gewährleistet eine genaue und zuverlässige Analyse der Oberflächenmorphologie der trocknenden Farbe.

Morphologie der Lackoberfläche
Morphologie der Lackbeschichtung

ABBILDUNG 2: Entwicklung der Oberflächenmorphologie der trocknenden Farbe zu verschiedenen Zeitpunkten.

Charakterisierung von Lackoberflächen
Oberflächenprofil der Farbe
Analyse der Lackoberfläche

ABBILDUNG 3: 3D-Ansicht der Entwicklung der Lackoberfläche bei verschiedenen Trocknungszeiten.

Oberflächenprofilometrie von Lackierungen

ABBILDUNG 4: 2D-Profil über der Lackprobe nach verschiedenen Trocknungszeiten.

Untersuchung der Lackoberfläche

ABBILDUNG 5: Entwicklung der durchschnittlichen Probenhöhe und des Rauhigkeitswerts Sa in Abhängigkeit von der Trocknungszeit des Lacks.

ISO 25178 – Oberflächenstrukturparameter

Trocknungszeit (min) 0 5 10 20 30 40 50 60
Sq (µm) 7.91 9.4 10.8 20.9 22.6 20.6 19.9 19.6
Sku 26.3 19.8 14.6 11.9 10.5 9.87 9.83 9.82
Sp (µm) 97.4 105 108 116 125 118 114 112
Sv (µm) 127 70.2 116 164 168 138 130 128
Sz (µm) 224 175 224 280 294 256 244 241
Sa (µm) 4.4 5.44 6.42 12.2 13.3 12.2 11.9 11.8

Sq - Wurzel-Mittel-Quadrat-Höhe | Sku - Kurtosis | Sp - Maximale Peakhöhe | Sv - Maximale Grubenhöhe | Sz - Maximale Höhe | Sv - Arithmetisches Mittel der Höhe

TABELLE 1: Rauheit der Farbe bei unterschiedlichen Trocknungszeiten.

SCHLUSSFOLGERUNG

In dieser Anwendung haben wir die Fähigkeiten des berührungslosen 3D-Profilometers NANOVEA ST500 bei der Überwachung der Entwicklung der Oberflächenmorphologie von Lacken während des Trocknungsprozesses demonstriert. Der optische Hochgeschwindigkeits-Zeilensensor, der eine Linie mit 192 Lichtpunkten erzeugt, die die Probenoberfläche gleichzeitig abtasten, hat die Untersuchung zeitsparend gemacht und gleichzeitig eine unübertroffene Genauigkeit gewährleistet.

Die Makrofunktion der Erfassungssoftware ermöglicht die Programmierung automatischer Messungen der 3D-Oberflächenmorphologie in situ, was besonders für Langzeitmessungen mit mehreren Scans in bestimmten Zeitintervallen nützlich ist. Dies reduziert den Zeit- und Arbeitsaufwand sowie das Potenzial für Benutzerfehler erheblich. Die fortschreitenden Veränderungen der Oberflächenmorphologie werden kontinuierlich überwacht und in Echtzeit aufgezeichnet, während die Farbe trocknet, was wertvolle Einblicke in den Trocknungsmechanismus der Farbe ermöglicht.

Die hier gezeigten Daten stellen nur einen Bruchteil der in der Analysesoftware verfügbaren Berechnungen dar. NANOVEA Profilometer sind in der Lage, praktisch jede Oberfläche zu messen, egal ob sie transparent, dunkel, reflektierend oder undurchsichtig ist.

Progressive Abnutzung von Bodenbelägen mit Tribometer

Prüfung der Abriebfestigkeit von Bodenbelägen

Progressive Verschleißkartierung von Bodenbelägen unter Verwendung eines Tribometers mit integriertem Profilometer

Prüfung der Abriebfestigkeit von Bodenbelägen

Vorbereitet von

FRANK LIU

EINFÜHRUNG

Bodenbeläge sind auf Langlebigkeit ausgelegt, unterliegen jedoch häufig der Abnutzung durch alltägliche Aktivitäten wie Bewegung und Möbelnutzung. Um ihre Langlebigkeit zu gewährleisten, verfügen die meisten Bodenbeläge über eine schützende Nutzschicht, die Beschädigungen widersteht. Die Dicke und Haltbarkeit der Nutzschicht variiert jedoch je nach Bodenbelagsart und Beanspruchungsgrad. Darüber hinaus weisen verschiedene Schichten innerhalb der Bodenbelagsstruktur, wie UV-Beschichtungen, Dekorschichten und Glasuren, unterschiedliche Abnutzungsraten auf. Hier kommt die progressive Verschleißkartierung ins Spiel. Mit dem NANOVEA T2000 Tribometer mit integriertem 3D berührungsloses ProfilometerEine präzise Überwachung und Analyse der Leistung und Langlebigkeit von Bodenbelagsmaterialien ist möglich. Durch detaillierte Einblicke in das Abnutzungsverhalten verschiedener Bodenbelagsmaterialien können Wissenschaftler und Techniker fundiertere Entscheidungen bei der Auswahl und Gestaltung neuer Bodenbelagssysteme treffen.

BEDEUTUNG DER PROGRESSIVEN VERSCHLEISSABBILDUNG FÜR BODENPLATTEN

Bei der Prüfung von Bodenbelägen wird traditionell die Abnutzungsrate einer Probe untersucht, um ihre Beständigkeit gegen Verschleiß zu bestimmen. Mit der progressiven Abnutzungskartierung kann jedoch die Abnutzungsrate der Probe während des gesamten Tests analysiert werden, was wertvolle Einblicke in das Abnutzungsverhalten liefert. Diese eingehende Analyse ermöglicht Korrelationen zwischen Reibungsdaten und Verschleißrate, wodurch die Grundursachen des Verschleißes ermittelt werden können. Es ist zu beachten, dass die Verschleißraten bei Verschleißtests nicht konstant sind. Die Beobachtung des Verschleißverlaufs ermöglicht daher eine genauere Beurteilung des Verschleißes der Probe. Die Einführung der progressiven Abnutzungskartierung hat über die traditionellen Prüfmethoden hinaus zu bedeutenden Fortschritten auf dem Gebiet der Bodenbelagsprüfung beigetragen.

Das NANOVEA T2000 Tribometer mit integriertem berührungslosen 3D-Profilometer ist eine bahnbrechende Lösung für Verschleißtests und Volumenverlustmessungen. Seine Fähigkeit, sich präzise zwischen dem Stift und dem Profilometer zu bewegen, garantiert die Zuverlässigkeit der Ergebnisse, indem es Abweichungen im Radius oder in der Position der Verschleißspur eliminiert. Aber das ist noch nicht alles – die erweiterten Funktionen des 3D-Berührungslos-Profilometers ermöglichen Hochgeschwindigkeits-Oberflächenmessungen und reduzieren die Scanzeit auf nur wenige Sekunden. Mit der Fähigkeit, Lasten von bis zu 2.000 N aufzubringen und Schleudergeschwindigkeiten von bis zu 5.000 U/min zu erreichen, ist die NANOVEA T2000 Tribometer bietet Vielseitigkeit und Präzision im Bewertungsprozess. Es ist klar, dass diese Ausrüstung eine entscheidende Rolle bei der Kartierung des fortschreitenden Verschleißes spielt.

 
Prüfung der Abriebfestigkeit von Bodenbelägen mit einem Tribometer
Prüfung der Abriebfestigkeit von Bodenbelägen mit einem Profilometer

ABBILDUNG 1: Aufbau der Probe vor der Verschleißprüfung (links) und Profilometrie der Abnutzungsspur nach der Prüfung (rechts).

MESSZIEL

Progressive Verschleißtests wurden an zwei Arten von Bodenbelägen durchgeführt: Stein und Holz. Jede Probe wurde insgesamt 7 Testzyklen mit ansteigender Testdauer von 2, 4, 8, 20, 40, 60 und 120 Sekunden unterzogen, um einen Vergleich der Abnutzung über die Zeit zu ermöglichen. Nach jedem Testzyklus wurde die Verschleißspur mit dem berührungslosen 3D-Profilometer NANOVEA profiliert. Anhand der vom Profilometer erfassten Daten können das Volumen des Lochs und die Verschleißrate mit den integrierten Funktionen der NANOVEA Tribometer-Software oder unserer Oberflächenanalyse-Software Mountains analysiert werden.

NANOVEA T2000 Hohe Belastung
Pneumatisches Tribometer

DIE MUSTER

wear mapping test samples Holz und Stein

PARAMETER DER VERSCHLEISSABBILDUNGSTESTS

LOAD40 N
TESTDAUERvariiert
SPEED200 Umdrehungen pro Minute
RADIUS10 mm
DISTANZvariiert
KUGELMATERIALWolframkarbid
KUGEL-DIAMETER10 mm

Die Testdauer für die 7 Zyklen betrug 2, 4, 8, 20, 40, 60 und 120 Sekundenjeweils. Die zurückgelegten Entfernungen waren 0,40, 0,81, 1,66, 4,16, 8,36, 12,55 und 25,11 Meter.

ERGEBNISSE DER VERSCHLEISSKARTIERUNG

Holzboden

Test-ZyklusMax COFMin COFAvg. COF
10.3350.1240.275
20.3370.2070.295
30.3800.2290.329
40.3930.2650.354
50.3520.2050.314
60.3450.1990.312
70.3150.2110.293

 

RADIALE ORIENTIERUNG

Test-ZyklusGesamtvolumenverlust (µm3)Gesamtabstand
Zurückgelegte Strecke (m)
Abnutzungsrate
(mm/Nm) x10-5
Momentane Verschleißrate
(mm/Nm) x10-5
12962476870.401833.7461833.746
23552452271.221093.260181.5637
35963713262.88898.242363.1791
48837477677.04530.629172.5496
5120717995115.40360.88996.69074
6147274531827.95293.32952.89311
7185131921053.06184.34337.69599
Progressiver Holzverschleiß im Vergleich zur Gesamtstrecke
Abnutzungsrate von Holzböden

ABBILDUNG 2: Verschleißrate im Vergleich zur zurückgelegten Gesamtstrecke (links)
und momentane Abnutzungsrate im Vergleich zum Testzyklus (rechts) für Holzfußböden.

Prüfung des Reibungskoeffizienten von Bodenbelägen
Kartierung der progressiven Abnutzung von Holzböden

ABBILDUNG 3: COF-Diagramm und 3D-Ansicht der Abnutzungsspur von Test #7 auf Holzfußboden.

Verschleißabbildung extrahiertes Profil
Ergebnisse der Abriebtests für Bodenbeläge
Charakterisierung von Bodenbelägen

ABBILDUNG 4: Querschnittsanalyse der Holzabriebspur aus Test #7

Progressive Verschleißkartierung Volumen- und Flächenanalyse

ABBILDUNG 5: Volumen- und Flächenanalyse der Abnutzungsspur an der Holzprobe #7.

ERGEBNISSE DER VERSCHLEISSKARTIERUNG

Steinboden

Test-ZyklusMax COFMin COFAvg. COF
10.2490.0350.186
20.3490.1970.275
30.2940.1540.221
40.5030.1240.273
50.5480.1060.390
60.5100.1290.434
70.5270.1810.472

 

RADIALE ORIENTIERUNG

Test-ZyklusGesamtvolumenverlust (µm3)Gesamtabstand
Zurückgelegte Strecke (m)
Abnutzungsrate
(mm/Nm) x10-5
Momentane Verschleißrate
(mm/Nm) x10-5
1962788460.40595.957595.9573
28042897311.222475.1852178.889
313161478552.881982.355770.9501
431365302157.041883.2691093.013
51082173218015.403235.1802297.508
62017496034327.954018.2821862.899
74251206342053.064233.0812224.187
Verschleißrate von Steinböden im Vergleich zur Entfernung
Diagramm für die momentane Abnutzungsrate von Steinböden

ABBILDUNG 6: Verschleißrate im Vergleich zur zurückgelegten Gesamtstrecke (links)
und momentane Abnutzungsrate im Vergleich zum Testzyklus (rechts) für Steinböden.

Tribologische Prüfung der Abriebfestigkeit von Bodenbelägen
Steinboden 3d Profil der Verschleißspur

ABBILDUNG 7: COF-Diagramm und 3D-Ansicht der Abnutzungsspur von Test #7 auf Steinboden.

Steinböden mit progressivem Verschleiß, extrahiertes Profil
Steinböden extrahiert Profil maximale Tiefe und Höhe Bereich des Lochs und Spitze
Tribologische Prüfung von Bodenbelägen

ABBILDUNG 8: Querschnittsanalyse der Steinverschleißspur von Test #7.

Volumenanalyse der fortschreitenden Abnutzung von Holzböden

ABBILDUNG 9: Volumen- und Flächenanalyse der Abnutzungsspur an der Steinprobe #7.

DISKUSSION

Die momentane Verschleißrate wird mit der folgenden Gleichung berechnet:
Abbildung der progressiven Abnutzung der Bodenbelagsformel

Diese Gleichung beschreibt die Verschleißrate zwischen den Prüfzyklen, wobei V das Volumen eines Lochs, N die Last und X die Gesamtstrecke ist. Die momentane Abnutzungsrate kann verwendet werden, um Änderungen der Abnutzungsrate während des Tests besser zu erkennen.

Beide Proben weisen ein sehr unterschiedliches Abnutzungsverhalten auf. Im Laufe der Zeit beginnt der Holzboden mit einer hohen Abnutzungsrate, sinkt aber schnell auf einen kleineren, gleichmäßigen Wert. Bei den Steinböden scheint die Abnutzungsrate bei einem niedrigen Wert zu beginnen und im Laufe der Zyklen auf einen höheren Wert zu steigen. Auch die momentane Abnutzungsrate zeigt wenig Konstanz. Der genaue Grund für den Unterschied ist nicht sicher, könnte aber auf die Struktur der Proben zurückzuführen sein. Der Steinboden scheint aus losen, kornähnlichen Partikeln zu bestehen, die sich anders abnutzen als die kompakte Struktur des Holzes. Um die Ursache für dieses Abnutzungsverhalten herauszufinden, wären weitere Tests und Untersuchungen erforderlich.

Die Daten des Reibungskoeffizienten (COF) scheinen mit dem beobachteten Verschleißverhalten übereinzustimmen. Die COF-Kurve für den Holzfußboden scheint über die Zyklen hinweg konsistent zu sein, was die gleichmäßige Verschleißrate ergänzt. Bei den Steinböden steigt der durchschnittliche COF über die Zyklen hinweg an, ähnlich wie die Verschleißrate mit den Zyklen zunimmt. Es gibt auch offensichtliche Veränderungen in der Form der Reibungskurven, was auf Veränderungen in der Wechselwirkung zwischen der Kugel und der Steinprobe hindeutet. Am deutlichsten ist dies in Zyklus 2 und Zyklus 4.

SCHLUSSFOLGERUNG

Das NANOVEA T2000 Tribometer zeigt seine Fähigkeit, progressiven Verschleiß zu kartieren, indem es die Verschleißrate zwischen zwei verschiedenen Bodenbelagsproben analysiert. Die Unterbrechung des kontinuierlichen Verschleißtests und das Scannen der Oberfläche mit dem berührungslosen NANOVEA 3D-Profilometer liefert wertvolle Erkenntnisse über das Verschleißverhalten des Materials im Laufe der Zeit.

Das NANOVEA T2000 Tribometer mit dem integrierten berührungslosen 3D-Profilometer liefert eine Vielzahl von Daten, darunter COF-Daten (Reibungskoeffizient), Oberflächenmessungen, Tiefenmessungen, Oberflächenvisualisierung, Volumenverlust, Verschleißrate und mehr. Diese umfassenden Informationen ermöglichen dem Benutzer ein tieferes Verständnis der Wechselwirkungen zwischen dem System und der Probe. Mit seiner kontrollierten Belastung, der hohen Präzision, der einfachen Bedienung, der hohen Belastung, dem großen Geschwindigkeitsbereich und den zusätzlichen Umgebungsmodulen hebt das NANOVEA T2000 Tribometer die Tribologie auf ein neues Niveau.

Rauheitskartierung mit 3D-Profilometrie

PRÜFUNG DER RAUHEITSKARTIERUNG

3D-PROFILOMETRIE VERWENDEN

Vorbereitet von

DUANJIE, PhD

EINFÜHRUNG

Oberflächenrauheit und -beschaffenheit sind entscheidende Faktoren, die sich auf die endgültige Qualität und Leistung eines Produkts auswirken. Ein gründliches Verständnis von Oberflächenrauheit, -textur und -konsistenz ist für die Auswahl der besten Verarbeitungs- und Kontrollmaßnahmen unerlässlich. Eine schnelle, quantifizierbare und zuverlässige Inline-Inspektion von Produktoberflächen ist notwendig, um fehlerhafte Produkte rechtzeitig zu erkennen und die Bedingungen in der Produktionslinie zu optimieren.

BEDEUTUNG DES BERÜHRUNGSLOSEN 3D-PROFILOMETERS FÜR DIE INLINE-OBERFLÄCHENPRÜFUNG

Oberflächenfehler an Produkten entstehen durch Materialverarbeitung und Produktherstellung. Die Inline-Oberflächenqualitätsprüfung gewährleistet eine strengste Qualitätskontrolle der Endprodukte. NANOVEA Berührungslose optische 3D-Profiler Nutzen Sie die Chromatic Light-Technologie mit der einzigartigen Fähigkeit, die Rauheit einer Probe berührungslos zu bestimmen. Der Zeilensensor ermöglicht das Scannen des 3D-Profils einer großen Oberfläche mit hoher Geschwindigkeit. Der von der Analysesoftware in Echtzeit berechnete Rauheitsschwellenwert dient als schnelles und zuverlässiges Gut/Schlecht-Instrument.

MESSZIEL

In dieser Studie wird das mit einem Hochgeschwindigkeitssensor ausgestattete NANOVEA ST400 zur Inspektion der Oberfläche einer Teflon-Probe mit einem Defekt verwendet, um die Fähigkeiten des NANOVEA

Berührungslose Profilometer ermöglichen eine schnelle und zuverlässige Oberflächenprüfung in einer Produktionslinie.

NANOVEA

ST400

ERGEBNISSE & DISKUSSION

3D-Oberflächenanalyse des Rauhigkeit Standardprobe

Die Oberfläche eines Rauheitsnormals wurde mit einem NANOVEA ST400 abgetastet, der mit einem Hochgeschwindigkeitssensor ausgestattet ist, der eine helle Linie mit 192 Punkten erzeugt, wie in ABBILDUNG 1 dargestellt. Diese 192 Punkte tasten die Probenoberfläche gleichzeitig ab, was zu einer deutlich höheren Abtastgeschwindigkeit führt.

ABBILDUNG 2 zeigt Falschfarbenansichten der Oberflächenhöhenkarte und der Rauheitsverteilungskarte der Rauheitsstandardprobe. In ABBILDUNG 2a weist der Rauheitsstandard eine leicht schräge Oberfläche auf, die durch den unterschiedlichen Farbverlauf in jedem der Standard-Rauheitsblöcke dargestellt wird. In ABBILDUNG 2b wird eine homogene Rauheitsverteilung in verschiedenen Rauheitsblöcken gezeigt, deren Farbe die Rauheit in den Blöcken darstellt.

ABBILDUNG 3 zeigt Beispiele für die Pass/Fail-Karten, die von der Analysesoftware auf der Grundlage verschiedener Rauheitsschwellenwerte erstellt wurden. Die Rauheitsblöcke werden rot hervorgehoben, wenn ihre Oberflächenrauheit über einem bestimmten Schwellenwert liegt. Auf diese Weise kann der Benutzer einen Rauheitsschwellenwert festlegen, um die Qualität der Oberflächenbeschaffenheit einer Probe zu bestimmen.

ABBILDUNG 1: Abtastung des optischen Zeilensensors auf der Probe des Rauheitsnormals

a. Karte der Oberflächenhöhe:

b. Rauhigkeitskarte:

ABBILDUNG 2: Falschfarbenansichten der Oberflächenhöhenkarte und der Rauheitsverteilungskarte der Rauheitsstandardprobe.

ABBILDUNG 3: Pass/Fail Map basierend auf dem Roughness Threshold.

Oberflächeninspektion einer Teflonprobe mit Defekten

Die Oberflächenhöhenkarte, die Rauheitsverteilungskarte und die Pass/Fail-Rauheitsschwellenkarte der Oberfläche der Teflon-Probe sind in ABBILDUNG 4 dargestellt. Die Teflon-Probe weist in der rechten Mitte der Probe eine Rippenform auf, wie in der Oberflächenhöhenkarte dargestellt.

a. Karte der Oberflächenhöhe:

Die verschiedenen Farben in der Palette von ABBILDUNG 4b stellen den Rauheitswert auf der lokalen Oberfläche dar. Die Rauhigkeitskarte zeigt eine homogene Rauheit im intakten Bereich der Teflon-Probe. Die Defekte in Form eines eingedrückten Rings und einer Verschleißnarbe sind jedoch in heller Farbe hervorgehoben. Der Benutzer kann leicht einen Schwellenwert für die Pass/Fail-Rauheit festlegen, um die Oberflächendefekte zu lokalisieren, wie in ABBILDUNG 4c gezeigt. Mit einem solchen Werkzeug kann der Benutzer die Oberflächenqualität des Produkts in der Produktionslinie vor Ort überwachen und fehlerhafte Produkte rechtzeitig erkennen. Der Echtzeit-Rauigkeitswert wird berechnet und aufgezeichnet, während die Produkte den optischen Inline-Sensor passieren, was als schnelles und zuverlässiges Werkzeug für die Qualitätskontrolle dienen kann.

b. Rauhigkeitskarte:

c. Pass/Fail Roughness Threshold Map:

ABBILDUNG 4: Oberflächenhöhenkarte, Rauhigkeitsverteilungskarte und Pass/Fail-Rauhigkeitsschwellenwertkarte der Teflon-Probenoberfläche.

SCHLUSSFOLGERUNG

In dieser Anwendung haben wir gezeigt, wie der berührungslose optische 3D-Profiler NANOVEA ST400, ausgestattet mit einem optischen Zeilensensor, als zuverlässiges Qualitätskontrollwerkzeug effektiv und effizient arbeitet.

Der optische Zeilensensor erzeugt eine helle Linie aus 192 Punkten, die die Probenoberfläche gleichzeitig abtasten, was zu einer deutlich höheren Abtastgeschwindigkeit führt. Er kann in der Produktionslinie installiert werden, um die Oberflächenrauhigkeit der Produkte vor Ort zu überwachen. Der Schwellenwert für die Rauheit dient als zuverlässiges Kriterium zur Bestimmung der Oberflächenqualität der Produkte und ermöglicht es dem Benutzer, fehlerhafte Produkte rechtzeitig zu erkennen.

Die hier gezeigten Daten stellen nur einen Teil der in der Analysesoftware verfügbaren Berechnungen dar. NANOVEA Profilometer messen praktisch jede Oberfläche in Bereichen wie Halbleiter, Mikroelektronik, Solar, Faseroptik, Automobil, Luft- und Raumfahrt, Metallurgie, Bearbeitung, Beschichtungen, Pharmazeutik, Biomedizin, Umwelt und vielen anderen.

Schweißnahtoberflächeninspektion mit einem tragbaren 3D-Profilometer

WELd-Oberflächeninspektion

Verwendung eines tragbaren 3d-Profilometers

Vorbereitet von

CRAIG LEISING

EINFÜHRUNG

Es kann von entscheidender Bedeutung sein, dass eine bestimmte Schweißnaht, die in der Regel durch eine Sichtprüfung erfolgt, mit einem extremen Präzisionsgrad untersucht wird. Zu den spezifischen Bereichen, die für eine präzise Analyse von Interesse sind, gehören Oberflächenrisse, Porosität und ungefüllte Krater, unabhängig von den nachfolgenden Prüfverfahren. Schweißnahtmerkmale wie Abmessungen/Form, Volumen, Rauheit, Größe usw. können zur kritischen Bewertung gemessen werden.

BEDEUTUNG DES BERÜHRUNGSLOSEN 3D-PROFILOMETERS FÜR DIE SCHWEISSNAHTOBERFLÄCHENPRÜFUNG

Im Gegensatz zu anderen Techniken wie Touch Probes oder Interferometrie bietet die NANOVEA Berührungsloses 3D-ProfilometerMithilfe des axialen Chromatismus kann nahezu jede Oberfläche gemessen werden, die Probengröße kann aufgrund der offenen Bereitstellung stark variieren und es ist keine Probenvorbereitung erforderlich. Der Nano- bis Makrobereich wird während der Oberflächenprofilmessung ohne Einfluss des Probenreflexionsvermögens oder der Probenabsorption erzielt, verfügt über eine erweiterte Fähigkeit zur Messung großer Oberflächenwinkel und es gibt keine Softwaremanipulation der Ergebnisse. Messen Sie ganz einfach jedes Material: transparent, undurchsichtig, spiegelnd, diffus, poliert, rau usw. Die 2D- und 2D-Funktionen der tragbaren NANOVEA-Profilometer machen sie zu idealen Instrumenten für die vollständige Inspektion von Schweißoberflächen sowohl im Labor als auch vor Ort.

MESSZIEL

In dieser Anwendung wird der NANOVEA JR25 Portable Profiler verwendet, um die Oberflächenrauheit, die Form und das Volumen einer Schweißnaht sowie die Umgebung zu messen. Diese Daten können wichtige Informationen liefern, um die Qualität der Schweißnaht und des Schweißprozesses richtig zu untersuchen.

NANOVEA

JR25

TESTERGEBNISSE

Das Bild unten zeigt die vollständige 3D-Ansicht der Schweißnaht und des umgebenden Bereichs zusammen mit den Oberflächenparametern der Schweißnaht. Das 2D-Querschnittsprofil ist unten dargestellt.

die Probe

Mit dem obigen 2D-Querschnittsprofil, das aus dem 3D-Profil entfernt wurde, werden die Dimensionsinformationen der Schweißnaht unten berechnet. Oberfläche und Volumen des Materials werden nur für die Schweißnaht berechnet.

 HOLEPEAK
OBERFLÄCHE1,01 mm214,0 mm2
VOLUME8,799e-5 mm323,27 mm3
MAXIMALE TIEFE/HÖHE0,0276 mm0,6195 mm
MITTLERE TIEFE/HÖHE 0,004024 mm 0,2298 mm

SCHLUSSFOLGERUNG

In dieser Anwendung haben wir gezeigt, wie der berührungslose 3D-Profiler NANOVEA kritische Eigenschaften einer Schweißnaht und der sie umgebenden Oberfläche präzise charakterisieren kann. Anhand der Rauheit, der Abmessungen und des Volumens kann eine quantitative Methode für Qualität und Wiederholbarkeit bestimmt und weiter untersucht werden. Musterschweißnähte, wie das Beispiel in dieser App Note, können mit einem Standard-Tischgerät oder einem tragbaren NANOVEA Profiler für Inhouse- oder Feldtests leicht analysiert werden.