Application Note | Rock Tribology

Rock Abrasivity Testing of Marble and Limestone Using a Pin-on-Disk Tribometer

Comparing Friction, Wear Rate, and Hardness of Rock for Drilling, Mining, and Building Applications

Excavator with a hydraulic breaker working a rock face in a quarry

Research & Experimental Testing

Duanjie Li

Visual Design & Editorial

Andrew Shore

Introduction

Rocks are composed of grains of minerals. The type and abundance of these minerals, as well as the chemical bonding strength between the mineral grains, determine the mechanical and tribological properties of the rocks. Depending on the geological rock cycles, rocks can undergo transformations and are typically classified into three major types: igneous, sedimentary, and metamorphic. These rocks exhibit different mineral and chemical compositions, permeabilities, and particle sizes, and such characteristics contribute to their varied wear resistance. Rock tribology explores the wear and friction behaviors of rocks in various geological and environmental conditions.

A smooth white marble block beside a porous, beige limestone block
Marble and limestone samples compared in this rock abrasivity study.

Why Rock Abrasivity Testing Matters

Various types of wear against rocks, including abrasion and friction, occur during the drilling process of wells, leading to significant direct and consequential losses attributed to the repair and replacement of drill bits and cutting tools. Therefore, the study of drillability, boreability, cuttability, and abrasivity of rocks is critical in the oil, gas, and mining industries.

Rock tribology research plays a pivotal role in the selection of the most efficient and cost-effective drilling strategies, thereby enhancing overall efficiency and contributing to the conservation of materials, energy, and the environment. Additionally, minimizing surface friction is highly advantageous in reducing the interaction between the drilling bit and the rock, resulting in decreased tool wear and improved drilling and cutting efficiency.

Measurement Objective

This study simulates and compares the tribological properties of two types of rock, limestone and marble, to show how the NANOVEA T50 Tribometer measures the coefficient of friction and wear rate of rocks in a controlled and monitored manner.

The hardness and elastic modulus of both rocks were also measured.

NANOVEA T50 Compact

Free Weight Tribometer

NANOVEA T50 free weight tribometer for friction and wear testing

Measurement Principle

In a pin-on-disk wear test, a ball or pin is loaded onto the sample with a precisely known normal force while the sample rotates beneath it, so the counter material traces a circular wear track at a set radius. The friction force is recorded continuously throughout the test, giving the evolution of the coefficient of friction (COF) with sliding distance.

After the test, the cross-section of the wear track is measured with a non-contact optical profilometer. The worn volume, together with the normal load and the sliding distance, gives the specific wear rate of the material.

Test Procedure

The coefficient of friction and the wear resistance of the two rock samples were evaluated with the NANOVEA T50 Tribometer using its Pin-on-Disc Wear Module. An Al2O3 ball with a 6 mm diameter was used as the counter material. The test parameters are summarized in the table below.

The wear rate, K, was evaluated using the formula K = V/(F × s) = A/(F × n), where V is the worn volume, F is the normal load, s is the sliding distance, A is the cross-sectional area of the wear track, and n is the number of revolutions.

Surface roughness and wear track profiles were evaluated with a NANOVEA Optical Profilometer, and the wear track morphology was examined using an optical microscope. The hardness and elastic modulus of each rock were measured using the Micro Indentation module of a NANOVEA Mechanical Tester.

The Al2O3 ball was used as an example counter material in this study. Any solid material, in different shapes, can be applied using a custom fixture to simulate the actual application.

ParameterValue
SamplesLimestone, marble
Counter materialAl2O3 ball, 6 mm diameter
Wear ring radius5 mm
Normal force10 N
Test duration10 min
Speed100 rpm

Pin-on-disk wear test parameters used for the limestone and marble samples.

Results and Discussion

Hardness and Elastic Modulus

The hardness (H) and elastic modulus (E) of the limestone and marble samples, measured with the Micro Indentation module of the NANOVEA Mechanical Tester, are compared in Fig. 1. The limestone exhibited lower H and E values, at 0.53 GPa and 25.9 GPa respectively, while the marble recorded 1.07 GPa for H and 49.6 GPa for E.

The relatively higher variability in the H and E values of the limestone can be attributed to its greater surface inhomogeneity, stemming from its granulated and porous character.

Bar chart of hardness and Young's modulus for limestone (0.53 GPa, 25.9 GPa) and marble (1.07 GPa, 49.6 GPa), with error bars
Fig. 1: Hardness and Young’s modulus comparison between limestone and marble samples, measured by micro indentation.

Coefficient of Friction

The evolution of the COF during the wear tests of the two rock samples is shown in Fig. 2. The limestone experiences a rapid increase in COF to approximately 0.8 at the beginning of the wear test and maintains this value throughout the test. This abrupt change can be attributed to the penetration of the Al2O3 ball into the rock, resulting from rapid wear and roughening at the contact face within the wear track.

In contrast, the marble sample shows a notable increase in COF to higher values only after approximately 5 m of sliding distance, signifying its superior wear resistance compared to the limestone.

Coefficient of friction versus sliding distance for limestone and marble: limestone rises to about 0.8 almost immediately, while marble stays low until about 5 m of sliding
Fig. 2: Evolution of the coefficient of friction (COF) in limestone and marble samples during pin-on-disk wear tests.

Wear Track Analysis and Wear Rate

Fig. 3 compares cross-sectional profiles of the limestone and marble samples after the wear tests, and Table 1 summarizes the results of the wear track analysis. Fig. 4 shows the wear tracks of the samples under the optical microscope.

The wear track evaluation aligns with the COF evolution observation: the marble sample, which maintains a low COF for a longer period, exhibits a lower wear rate of 0.0046 mm³/(N·m), compared to 0.0353 mm³/(N·m) for the limestone. The superior mechanical properties of marble contribute to its better wear resistance than limestone.

The limestone wear track had a valley area of 35.3 ± 5.9 × 10⁴ µm² and a valley depth of 229 ± 24 µm; the marble wear track had a valley area of 4.6 ± 1.2 × 10⁴ µm² and a valley depth of 61 ± 15 µm (Table 1).

Wear track cross-section profiles showing a larger, deeper wear track on limestone than on marble
Fig. 3: Cross-section profiles of the limestone and marble wear tracks, measured by non-contact profilometry.
SampleValley area
(×10⁴ µm²)
Valley depth
(µm)
Wear rate
(mm³/N·m)
Limestone35.3 ± 5.9229 ± 240.0353
Marble4.6 ± 1.261 ± 150.0046

Table 1: Result summary of wear track analysis: valley area, valley depth and wear rate of limestone and marble.

Optical microscope images of the wear tracks on limestone, with a granular surface, and on marble, where the track appears as a curved white band
Fig. 4: Limestone and marble wear tracks under an optical microscope.

Conclusion

This study showed how the NANOVEA Tribometer evaluates the coefficient of friction and wear resistance of two rock samples, marble and limestone, in a controlled and monitored manner.

The marble was harder and stiffer than the limestone (H 1.07 GPa and E 49.6 GPa, against 0.53 GPa and 25.9 GPa), kept a low coefficient of friction for about the first 5 m of sliding, and wore at 0.0046 mm³/(N·m), roughly 7.7 times more slowly than the limestone at 0.0353 mm³/(N·m).

The superior mechanical properties of marble contribute to its exceptional wear resistance. This property makes it challenging to drill or cut in the oil and gas industry. Conversely, it significantly extends its lifetime when used as a high-quality building material, such as floor tiles.

NANOVEA Tribometers offer precise and repeatable wear and friction testing to ISO and ASTM standards in both rotative and linear modes, with optional modules for high-temperature wear, lubrication, and tribocorrosion integrated in one system. Together with NANOVEA optical profilometers and mechanical testers, they characterize the full range of tribological properties of rocks, as well as thin or thick, soft or hard coatings, films, and substrates.

Frequently Asked Questions About Rock Abrasivity and Rock Tribology Testing

What is rock abrasivity, and how is it measured?

Rock abrasivity describes how strongly a rock wears the tools that drill, bore or cut it. It is commonly ranked with the CERCHAR test (ASTM D7625), in which a steel stylus is scratched across the rock and its wear is measured. A pin-on-disk tribometer test approaches the same contact from the rock side: it measures the rock's coefficient of friction and wear rate against a defined counter material, under controlled load, speed and sliding distance.

How is the wear rate of a rock calculated in a pin-on-disk test?

The specific wear rate is K = V / (F × s), where V is the worn volume, F the normal load and s the sliding distance, usually reported in mm³/(N·m). For a circular track of constant cross-section it simplifies to K = A / (F × n), with A the cross-sectional area of the wear track and n the number of revolutions. The track profile is measured with a non-contact optical profilometer.

Why did limestone wear faster than marble in this study?

The study attributes marble's better wear resistance to its superior mechanical properties: a hardness of 1.07 GPa and an elastic modulus of 49.6 GPa, against 0.53 GPa and 25.9 GPa for the limestone. Under the same test conditions the limestone wore at 0.0353 mm³/(N·m), roughly 7.7 times the marble's 0.0046 mm³/(N·m), and its friction rose to about 0.8 almost immediately as the ball penetrated and roughened the track.

What does the coefficient of friction reveal during a rock wear test?

Changes in friction show when and how the contact changes. The limestone's COF rose almost immediately to about 0.8 as the ball penetrated and roughened the track, while the marble kept a low COF for roughly the first 5 m of sliding before rising. Recording COF continuously therefore shows not only the final friction level but how long a surface resists wear.

Can the counter material simulate a drill bit or cutting tool?

Yes. The 6 mm Al2O3 ball in this study is one example. Any solid material, in different shapes, can be mounted with a custom fixture to reproduce the contact of a specific drill bit, cutter or tool material, and load, speed and environment can be set to approach field conditions.

Which NANOVEA instruments are used for rock tribology testing?

Friction and wear are measured with a NANOVEA Tribometer, such as the T50 with its pin-on-disk (rotational) module. The wear-track cross-section and wear volume are measured with a NANOVEA non-contact optical profilometer, and hardness and elastic modulus with the micro indentation module of a NANOVEA Mechanical Tester.