Application Note | Optical Component Inspection

Fresnel Lens Topography Using a 3D Non-Contact Optical Profilometer

Measuring Ring Height and Pitch of a Serrated Lens Profile to Catch Worn Molds and Stamps

Lighthouse at dusk, an application of Fresnel lenses

Research & Experimental Testing

Duanjie Li & Benjamin Mell

Visual Design & Editorial

Andrew Shore

Introduction

A lens is an optical device of axial symmetry that transmits and refracts light. A simple lens consists of a single optical component for converging or diverging the light. Even though spherical surfaces are not ideal shape for making a lens, they are often used as the simplest shape which glass can be ground and polished to.

A Fresnel lens consists of a series of concentric rings, which are thin parts of a simple lens with a width as small as a few thousandths of an inch. Fresnel lenses contain a large aperture and short focal length, with a compact design reducing the weight and volume of material required, compared to conventional lenses with the same optical properties. A very small amount of light is lost by absorption due to the thin geometry of the Fresnel lens.

Why 3D Non-Contact Profilometry Matters for Fresnel Lens Inspection

Fresnel lenses are extensively employed in the automotive industry, lighthouses, solar energy and optical landing systems for aircraft carriers. Molding or stamping the lenses out of transparent plastics can make their production cost-effective. Service quality of Fresnel lenses mostly depends on the precision and surface quality of their concentric ring. Unlike a touch probe technique, NANOVEA Optical Profilers perform 3D surface measurements without touching the surface, avoiding the risk of making new scratches. The Chromatic Light technique is ideal for precise scanning of complex shapes, such as lenses of different geometries.

Fresnel Lens Schematic

Fresnel lens schematic: front view with overall size, width and length, and side view of the serrated profile focusing light at the focal length
Fresnel lens schematic.

Transparent plastic Fresnel lenses can be manufactured by molding or stamping. Accurate and efficient quality control is critical to reveal defective production molds or stamps. By measuring the height and pitch of the concentric rings, production variations can be detected by comparing the measured values against the specification values given by the manufacturer of the lens.

Precise measurement of the lens profile ensures that the molds or stamps are properly machined to fit manufacturer specifications. Moreover, the stamp could progressively wear out over time, causing it to lose its initial shape. Consistent deviation from the lens manufacturer specification is a positive indication that the mold needs to be replaced.

Measurement Objective

In this application, we showcase NANOVEA ST400, a 3D Non-Contact Profiler with a high-speed sensor, providing comprehensive 3D profile analysis of an optical component of a complex shape. To demonstrate the remarkable capabilities of our Chromatic Light technology, the contour analysis is performed on a Fresnel lens.

NANOVEA ST400 Standard

Optical 3D Profilometer

NANOVEA ST400 modular optical profilometer for non-contact 3D surface measurement

Results

The 2.3” x 2.3” acrylic Fresnel lens used for this study consists of a series of concentric rings and a complex serrated cross-section profile. It has a 1.5” focal length, 2.0” effective size diameter, 125 grooves per inch, and an index of refraction of 1.49.

The NANOVEA ST400 scan of the Fresnel lens shows a noticeable increase in height of the concentric rings, moving outward from the center.

Lens specificationValue
MaterialAcrylic
Size2.3 in × 2.3 in
Focal length1.5 in
Effective size diameter2.0 in
Grooves per inch125
Index of refraction1.49

Table 1: Specifications of the Fresnel lens studied.

False-color height map of the Fresnel lens over about 9.5 mm, with concentric rings around the center
3D view of the Fresnel lens with its concentric rings rising toward the edge

Fig. 1: 2D false color height representation (left) and 3D view (right).

Serrated profile extracted across the Fresnel lens over 0.5 in, deepest at the center
Fig. 2: Extracted profile (length 0.5 in, Pt 2.572 mil).
Peak and valley dimensional analysis of the Fresnel lens profile with five measured ring pairs
Fig. 3: Peak and valley: dimensional analysis of the profile.
PairHorizontal distance (in)Height difference (mil)Slope (mil/in)Angle
0–10.0077952.445313.617.41°
2–30.007662.193286.315.98°
4–50.0070231.853263.814.78°
6–70.0074091.589214.512.11°
8–90.006251.248199.811.3°

Table 2: Ring pitch and height from the peak and valley analysis.

Conclusion

In this application, we have showcased that the NANOVEA ST400 non-contact Optical Profiler accurately measures the surface topography of Fresnel lenses.

The dimension of the height and pitch can be accurately determined from the complex serrated profile using NANOVEA analysis software. Users can effectively inspect the quality of the production molds or stamps by comparing the ring height and pitch dimensions of manufactured lenses against the ideal ring specification.

The data shown here represents only a portion of the calculations available in the analysis software. NANOVEA Optical Profilers measure virtually any surface in fields including Semiconductors, Microelectronics, Solar, Fiber Optics, Automotive, Aerospace, Metallurgy, Machining, Coatings, Pharmaceutical, Biomedical, Environmental and many others.

Frequently Asked Questions About Fresnel Lens Inspection

What is a Fresnel lens?

A Fresnel lens consists of a series of concentric rings, thin parts of a simple lens with widths as small as a few thousandths of an inch. It offers a large aperture and short focal length in a compact design that reduces the weight and material of a conventional lens with the same optical properties.

Why inspect Fresnel lens topography?

Service quality mostly depends on the precision and surface quality of the concentric rings. Measuring ring height and pitch against the manufacturer’s specification reveals defective molds or stamps, and consistent deviation indicates a mold or stamp has worn and needs replacement.

Why measure lenses without contact?

A touch probe risks making new scratches on the optical surface. NANOVEA optical profilers measure in 3D without touching the surface, and the chromatic light technique is ideal for precise scanning of complex shapes such as lenses of different geometries.

What does a Fresnel lens scan show?

For the 2.3 in × 2.3 in acrylic lens studied (1.5 in focal length, 125 grooves per inch), the scan shows the concentric rings increasing in height moving outward from the center, with a complex serrated cross-section profile.

How are ring height and pitch measured?

A profile is extracted across the rings and analyzed peak to valley. Here the first measured ring pair spanned 0.007795 in horizontally with a 2.445 mil height difference, a slope of 313.6 mil/in and an angle of 17.41°.

Which NANOVEA instrument was used for Fresnel lens inspection?

The NANOVEA ST400 3D Non-Contact Profiler with a high-speed chromatic light sensor. NANOVEA optical profilers measure surfaces across fields from semiconductors and fiber optics to automotive and aerospace.

Need Reliable Optical Component Inspection?