Application Note | Dynamic Mechanical Analysis
Dynamic Mechanical Analysis (DMA) Frequency Sweep on Polymer
Viscoelastic Behavior of Tire Rubber from 0.1 to 20 Hz in a Single Test

Research & Experimental Testing
Duanjie Li
Visual Design & Editorial
Andrew Shore
Introduction
Viscoelastic materials exhibit both viscous and elastic characteristics when undergoing deformation. Long molecular chains in polymer materials contribute to their unique viscoelastic properties, i.e. a combination of the characteristics of both elastic solids and Newtonian fluids. Stress, temperature, frequency and other factors all play roles in the viscoelastic properties. Dynamic Mechanical Analysis, also known as DMA, studies the viscoelastic behavior and complex modulus of a material by applying a sinusoidal stress and measuring the change of strain.
Importance of the Dynamic Mechanical Analysis Frequency Sweep Test
The changing frequency of the stress often leads to variations in the complex modulus, which is a critical mechanical property of polymers. For example, tires are subjected to cyclical high deformations when vehicles are running on the road. The frequency of the pressure and deformation changes as the car accelerates to higher speeds. Such a change can result in variation in the viscoelastic properties of the tire, which are important factors in the car’s performance. A reliable and repeatable test of the viscoelastic behavior of polymers at different frequencies is needed. The Nano module of the NANOVEA Mechanical Tester generates a sinusoidal load with a high precision piezo actuator and directly measures the evolution of force and displacement using an ultrasensitive load cell and capacitor. The combination of easy setup and high accuracy makes it an ideal tool for DMA frequency sweeps.
ℹ️ Learn more about nanoindentation and DMA lab services.
Measurement Objective
In this application, we study the viscoelastic properties of a polished tire sample at different DMA frequencies using the NANOVEA PB1000 Mechanical Tester in nanoindentation mode.
Test Conditions
| Parameter | Value |
|---|---|
| Frequencies | 0.1, 1, 5, 10, 20 Hz |
| Creep time at each frequency | 50 s |
| Oscillation voltage | 0.1 V |
| Loading voltage | 1 V |
| Indenter type | Spherical diamond, 100 µm |
Table 1: Test conditions.

Results and Discussion
The DMA frequency sweep at the maximum load allows a fast and simple measurement of the viscoelastic characteristics of the sample at different loading frequencies in one test. The phase shift and the amplitudes of the load and displacement waves at different frequencies can be used to calculate a variety of fundamental viscoelastic properties, including storage modulus, loss modulus and tan (δ), as summarized in the following graphs.
Frequencies of 1, 5, 10 and 20 Hz in this study correspond to speeds of about 7, 33, 67 and 134 km per hour. As the test frequency increases from 0.1 to 20 Hz, both storage modulus and loss modulus progressively increase. Tan (δ) decreases from ~0.27 to 0.18 as the frequency increases from 0.1 to 1 Hz, and then gradually increases to ~0.55 when the frequency of 20 Hz is reached. A DMA frequency sweep measures the trends of storage modulus, loss modulus and tan (δ), which provide information on the movement of the monomers and cross-linking as well as the glass transition of polymers. By raising the temperature with a heating plate during the frequency sweep, a more complete picture of the molecular motion under different test conditions can be obtained.



Conclusion
In this study, we showcased the capacity of the NANOVEA Mechanical Tester in performing a DMA frequency sweep on a tire sample. This test measures the viscoelastic properties of the tire at different stress frequencies. The tire shows increased storage and loss modulus as the loading frequency increases from 0.1 to 20 Hz. This provides useful information on the viscoelastic behavior of a tire running at different speeds, which is essential for improving tire performance for smoother and safer rides. The DMA frequency sweep can be performed at various temperatures to mimic the realistic working environment of the tire in different weather.
In the Nano module of the NANOVEA Mechanical Tester, load application by the fast piezo is independent of load measurement by a separate high-sensitivity strain gage. This gives a distinct advantage in DMA, since the phase between depth and load is measured directly from the sensor data. The phase calculation is direct and needs no mathematical modeling that would add inaccuracy to the resulting loss and storage modulus, which is not the case for a coil-based system.
In conclusion, DMA measures loss and storage modulus, complex modulus and tan (δ) as a function of contact depth, time and frequency, and an optional heating stage allows the phase transition temperature to be determined. The NANOVEA Mechanical Testers provide multi-function Nano and Micro modules on a single platform, both including scratch, hardness and wear tester modes.
Frequently Asked Questions About DMA Frequency Sweeps
What is dynamic mechanical analysis?
DMA applies a sinusoidal stress and measures the strain response to study the viscoelastic behavior and complex modulus of a material, which combines elastic-solid and viscous-fluid characteristics.
Why sweep the frequency?
Changing stress frequency changes the complex modulus; a tire, for example, deforms cyclically at a frequency that rises with vehicle speed, which affects its viscoelastic properties and the car’s performance.
How was the tire tested?
In nanoindentation mode with a 100 µm spherical diamond, at 0.1, 1, 5, 10 and 20 Hz, holding 50 s at each frequency, with a 1 V loading voltage and 0.1 V oscillation voltage.
What did the results show?
Storage and loss modulus both increased progressively from 0.1 to 20 Hz; tan δ fell from about 0.27 to 0.18 between 0.1 and 1 Hz, then rose to about 0.55 at 20 Hz.
What speeds do the frequencies represent?
Frequencies of 1, 5, 10 and 20 Hz correspond to about 7, 33, 67 and 134 km/h.
Why does the instrument design matter for DMA?
In the nano module the load is applied by a fast piezo and measured by a separate high-sensitivity sensor, so the phase between load and depth is measured directly rather than modeled, unlike coil-based systems.