Application Note | Nanoindentation DMA
Viscoelastic Analysis of Rubber
Mapping Tan δ, Storage and Loss Modulus Through the Layers of a Tire with Nanoindentation DMA

Research & Experimental Testing
NANOVEA Laboratory
Visual Design & Editorial
Andrew Shore
Introduction
Viscoelasticity is referred to as the property of materials that exhibit both viscous and elastic characteristics when undergoing deformation.
A viscous material resists shear flow and strains linearly with time when a stress is applied, unlike an elastic material that strains immediately when stressed and returns to original state once the stress is removed. A viscoelastic material exhibits elements of both properties and therefore has a complex modulus.
Importance of Nanoindentation DMA for Rubber
Tires are subjected to cyclical high deformations when vehicles are running on the road. When exposed to harsh road conditions, the service lifetime of the tires is jeopardized by many factors, such as the wear of the tread, the heat generated by friction, rubber aging, and others.
As a result, tires usually have composite layer structures made of carbon-filled rubber, nylon cords, and steel wires, etc. In particular, the composition of rubber at different areas of the tire systems is optimized to provide different functional properties, including but not limited to wear resistant tread, cushion rubber layer and hard rubber base layer.
A reliable and repeatable test of the viscoelastic behavior of rubber is critical in quality control and R&D of new tires, as well as evaluation of life span of old tires. Dynamic Mechanical Analysis (DMA) during Nanoindentation is a technique of characterizing the viscoelasticity. When controlled oscillatory stress is applied, the resulting strain is measured, allowing users to determine the complex modulus of the tested materials.
ℹ️ Learn more about nanoindentation and DMA lab services.

Tire rubber must perform under cyclical deformation and harsh road conditions.
Measurement Objective
In this application, the NANOVEA Mechanical Tester, in Nanoindentation mode with DMA is used to study the comparative viscoelastic properties of rubber at different thicknesses of a tire sample.

Testing Conditions
A series (40 points) of nanoindentation DMA was performed along the thickness of the tire sample and the distribution of the indentations is illustrated in Fig. 1. The test conditions are summarized in Table 1.
| Test parameter | Value |
|---|---|
| Maximum force | 75 mN |
| Loading rate | 150 mN/min |
| Creep | 20 s |
| Amplitude | 15 |
| Frequency | 10 Hz |
| Indenter type | 100 µm spherical diamond |
Table 1: Test conditions of the nanoindentation.

Results and Discussion
40 indentations along the tire thickness were performed spaced 0.38 mm apart for a total distance of ~15.5 mm as illustrated in Fig. 1 and the corresponding Tan (δ), Storage Modulus, Loss Modulus and Hardness measured from the DMA are summarized in Fig. 2 to Fig. 5.




The distribution of the hardness and complex modulus meets the functionality requirements of the rubber at different layers of the tires. The rubber at the positions from 0.38 to 2.66 mm and from 8.22 to 11.64 mm exhibits a relatively low hardness below 2 MPa and low complex modulus. Such a relative soft feature allows the rubber in these regions to serve as a cushion layer and absorb the shocks and vibrations. In comparison, the rubber at the positions from 3.04 to 7.84 mm shows an enhanced hardness and complex modulus, due to the composite structure consisting of reinforcing fabric or high tensile-strength steel wires encased in the rubber compound. The enhanced mechanical properties of this layer provide the tire structure strength and toughness. The positions from 12.02 to 15.82 mm reside in the tire tread and exhibit higher Hardness and complex modulus compared with the “cushion region”. The high carbon black concentration at this area gives reinforced abrasion resistance, cut resistance as well as traction.

Conclusion
In this study, we demonstrate how the NANOVEA Mechanical Tester in Nanoindentation DMA mode measures the viscoelastic properties of a rubber sample (used tire in this study). The profile seen across the depth of the tire shows how the different layers are used to create zones with very different behaviors. This is essential in tire design to decrease the vibration. Zones of high loss modulus will absorb differently than zones of low loss modulus. These types of studies are now essential to improve tires for smoother, safer rides that last as long as possible in different weather conditions. These tests can be performed at various temperatures and even under liquids. The test can also be conducted at various frequencies to mimic the behavior of tires as speed increases. Frequencies of 10Hz, used in this report, correspond to speed of about 67 km per hour. The NANOVEA DMA can go up to 100Hz and is also possible to scan across various frequencies to obtain a sweep.
The NANOVEA Mechanical Tester has true closed feedback control on load applied. The load application with the fast piezo is independent from the load measurement done by a separate high sensitivity strain gage. This gives a distinct advantage during DMA since the phase between depth and load is measured directly from the data collected from the sensor. The calculation of phase is direct and does not need mathematical modeling that adds inaccuracy to the resulting loss and storage modulus. This is not the case for coil systems.
In conclusion, DMA measures hardness, loss and storage modulus, complex modulus and Tan (δ) as a function of contact depth, time and frequency. The optional heating stage allows determination of materials phase transition temperature during DMA. The NANOVEA Mechanical Testers provide unmatched multifunction Nano and Micro/Macro modules on a single platform. Both the Nano and Micro/Macro modules include scratch tester, hardness tester and wear tester modes, providing the widest and most user friendly range of testing available on a single module.
Frequently Asked Questions About Nanoindentation DMA of Rubber
What is viscoelasticity?
The property of materials that show both viscous and elastic behavior when deformed. A viscous material strains linearly with time under stress, an elastic one strains immediately and recovers; a viscoelastic material does both and so has a complex modulus.
How does nanoindentation DMA work?
A controlled oscillatory stress is applied during nanoindentation and the resulting strain is measured, giving the complex modulus. Here it ran at 10 Hz with a 100 µm spherical diamond indenter to a maximum force of 75 mN.
Why test rubber across a tire’s thickness?
Tires are layered composites of carbon-filled rubber, nylon cords and steel wires, with rubber compositions optimized for each layer. A profile of 40 indentations, 0.38 mm apart, shows how each layer behaves.
What did the tire profile show?
Cushion layers at 0.38 to 2.66 mm and 8.22 to 11.64 mm had hardness below 2 MPa and low complex modulus; the reinforced layer at 3.04 to 7.84 mm and the tread at 12.02 to 15.82 mm were harder with higher complex modulus.
Can DMA simulate driving speed or temperature?
Tests can be run at various temperatures, even under liquids, and at various frequencies to mimic tires as speed increases; the 10 Hz used here corresponds to about 67 km per hour. The NANOVEA DMA reaches 100 Hz and can sweep frequencies.
Why does a separate load sensor matter for DMA?
Load is applied with a fast piezo and measured by a separate high-sensitivity strain gage, so the phase between depth and load is measured directly from the data, without modeling that adds inaccuracy to the loss and storage modulus.