Application Note | Scratch Depth
Micro Scratch Depth Using 3D Profilometry
Depth and Area of Micro Scratches in Seconds from One Line Scan

Research & Experimental Testing
Jorge Ramirez
Visual Design & Editorial
Andrew Shore
Introduction
Flaws such as scratches, texture, pits and dents are small changes in the surface of a product or raw material that might indicate a defect. Flaws can be consistent or random and can be difficult to detect by the human eye. It is critical not only to detect these defects but also to measure them at high speed with extreme precision, either during inline processing or in sample inspection during research. An example is the detection of micro scratches, where the measurement of depth and area is of critical interest.
Importance of 3D Non-Contact Profilometry for Scratch Depth
Using the 3D non-contact profilometer in 2D mode, the depth and area of micro scratches can be provided in seconds on nearly any material. If a 3D surface measurement is needed, the surface area can be selected, with speeds varying according to resolution and/or staging options. Detecting and controlling scratch flaws allows the best selection of processing and control measures, and assuring the quality control of such parameters relies heavily upon quantifiable, reproducible, reliable and fast inspection. The NANOVEA 3D Non-Contact Profilometers use axial chromatism, with a unique capability to measure nearly any material and the steep angles found in micro scratch measurement. Where other techniques fail to provide reliable data due to probe contact, surface variation, angle or reflectivity, NANOVEA Profilometers succeed.
ℹ️ Learn more about surface profiling lab services.
Measurement Objective
In this application, the NANOVEA ST400 Profilometer is used to measure a row of micro scratches created using the NANOVEA Mechanical Tester in scratch mode. In seconds, the profilometer provides depth and area measurements with a single line pass in 2D mode.

2D Results: Scratch Depth and Area
Scan parameters: X scan length 1.0, scan step size 1.0, 1001 points; Y scan length 2.2, profile step size 1.0, 2201 profiles; 2,203,201 points in total; pen setting 110, acquisition rate 200, averaging 1.

| Scratch | Maximum depth (µm) | Mean depth (µm) |
|---|---|---|
| 1 | 4.024 | 3.014 |
| 2 | 3.889 | 3.445 |
| 3 | 3.822 | 3.326 |
| 4 | 3.547 | 3.093 |
| 5 | 3.895 | 3.277 |
| 6 | 3.886 | 3.451 |
| 7 | 4.065 | 3.468 |
| 8 | 3.886 | 3.196 |
| 9 | 3.374 | 3.098 |
| 10 | 3.745 | 2.873 |
Table 1: Depth of the micro scratches (from Fig. 2).



Conclusion
In this application, we have shown how the NANOVEA ST400 3D Non-Contact Profilometer can precisely measure, in seconds, the depth and area of micro scratches with a single line scan. Other measurements available from a 2D single line scan include roughness, flatness, step height and many others. Together with predefined pass-fail parameters on these measurements, this creates a quick and repeatable analysis process. If a 3D surface measurement is needed, a full area can be measured and areas of interest quickly analyzed with a wide list of measurements (dimension, roughness, finish and texture, shape, form and topography, flatness, warpage and planarity, volume and area, step height and others).
NANOVEA 3D Profilometer speeds range from 20 mm/s to 1 m/s, from laboratory and research use to high-speed inspection; they can be built with custom sizes, speeds and scanning capabilities, Class 1 clean room compliance, an indexing conveyor and inline or online integration, and are also available as fully portable systems.
Frequently Asked Questions About Scratch Depth Measurement
Why measure micro scratch depth?
Scratches, pits and dents can indicate defects and are often hard to see; measuring their depth and area quickly and precisely matters for inline processing and research inspection.
How fast is the measurement?
A single line pass in 2D mode gives the depth and area of the scratches in seconds; a 3D area scan can be added when needed.
How deep were the scratches?
Maximum depths of the ten scratches ranged from 3.374 to 4.065 µm, with mean depths from 2.873 to 3.468 µm.
What cross-section areas were measured?
The combined hole area across the profile was 333.3 µm², and a single scratch measured 34.79 µm².
Can results be used for pass/fail?
Yes. Predefined pass-fail limits on depth, roughness, flatness or step height create a quick, repeatable analysis process.
Why is a non-contact profilometer suited to scratches?
Axial chromatism measures nearly any material and the steep flanks of micro scratches, where probe contact, angle or reflectivity defeat other techniques.