Application Note | Consumer Product Tribology

Brush Bristle Stiffness Performance Using Tribometer

Tracking Toothbrush Filament Bending and Fraying with the Tribometer Depth Sensor

Toothbrush head in toothpaste slurry on a tribometer

Research & Experimental Testing

Ali Mansouri

Visual Design & Editorial

Andrew Shore

Introduction

Brushes are among the most basic and widely used tools in the world. They can be used to remove material (toothbrush, archaeological brush, bench grinder brush), apply material (paintbrush, makeup brush, gilding brush), comb filaments, or add a pattern. As a result of the mechanical and abrasive forces on them, brushes constantly have to be replaced after moderate use. For example toothbrush heads should be replaced every three to four months because of fraying as a result of repeated usage. Making the toothbrush fiber filaments too stiff risks wearing away the actual tooth instead of soft plaque. Making the toothbrush fibers too soft makes the brush lose its form faster. Understanding the changing bend of the brush, as well as the wear and overall change in shape in the filaments under different loading conditions is necessary to design brushes that better fulfill their application.

Importance of Tribology Testing of Brush Stiffness

A reliable measurement of the brush bend is needed in order to be able to quantify the amount of brush fraying. This provides a useful tool to directly compare brush heads with different types of filaments and geometries. Tribology can provide important insights both about individual filaments and the brush system as a whole. Furthermore the effect of diverse lubricants, different loading conditions, and various brushed materials can be determined. The depth sensor can provide valuable information about the evolution of the filament-surface interface over time. These results can be applied to any solid-to-solid interface that loses its shape over time from abrasive or mechanical forces using a custom pin fixture.

ℹ️ Learn more about friction and wear testing lab services.

Measurement Objective

In this study, we showcase the capacity of the NANOVEA Tribometer for measuring the depth change of custom toothbrush fixtures with different stiffnesses against a smooth aluminum surface in the presence of a toothpaste slurry lubricant, which makes it an ideal tool for evaluating brush bending and wear under different loading conditions. The NANOVEA Tribometer can be customized to simulate a wide variety of different wear and friction conditions with various types of motion.

NANOVEA T2000 High Load

Pneumatic Tribometer

NANOVEA T2000 high load pneumatic tribometer
Toothbrush head pressed into toothpaste slurry in the tribometer lubrication cup
Fig. 1: Tribology measurement of a toothbrush head inside toothpaste slurry lubricant.

Test Procedure

A customized toothbrush head pin was created by attaching a standard toothbrush to a 10 mm steel ball that had been flattened on one side. This procedure could be used for any similarly sized object, in order to create a customized pin fixture. The brush was put in a lubrication cup that was filled with toothpaste slurry (as shown in Fig. 1). In this case, the brush was in contact with the bottom of the flat aluminum cup. The brush-ball system was tested using a linear reciprocating setup. The depth sensor was used to determine the vertical deflection of the toothbrush filaments at each point in the cycle. Two different brushes, with ‘soft’ and ‘firm’ stiffness were compared. The test parameters are summarized in Table 1.

ParameterValue
Load8 N
Test duration120 min
Speed100 rpm
Amplitude2 mm
Total distance48 m
PinToothbrush (soft, firm)
LubricantToothpaste slurry
Temperature24 °C

Table 1: Test parameters of the depth measurement.

Results and Discussion

The summary of the results of the two tests can be seen in Table 2. The test was conducted for two hours, which was the same as 48 meters of reciprocating linear wear. As expected, a much higher depth change was seen in the soft brush than the firm brush over the two hour interval. (The bend rate calculated here is an average over the entire test, whereas in reality, as will be seen from Fig. 5, the rate was much higher in the beginning of the test and slowed down as it progressed.)

SampleDepth change (mm)Bend rate × 10⁻⁴ (mm/Nm)
Firm brush0.1724.479
Soft brush0.2827.344

Table 2: Results of toothbrush depth measurements.

Fig. 2 and Fig. 3 show the evolution of brush depth over the course of the test for the firm and soft brush. There are two primary depth changes occurring here. Firstly, the brush filaments are being deflected from their normal positions over the course of each back and forth motion during each cycle. This is shown more clearly in Fig. 4.

Depth of the firm toothbrush over the two-hour test, oscillating each cycle and drifting upward
Fig. 2: Evolution of firm brush depth.
Depth of the soft toothbrush over the two-hour test
Fig. 3: Evolution of soft brush depth.
Zoomed section of the soft brush depth showing the oscillation in each reciprocating cycle
Fig. 4: Zoomed in portion of the soft brush plot.

At the same time, over the course of the test, the deflection of the brush filaments steadily increased. Comparing the same part of the back and forth reciprocating cycle over all 12,000 cycles shows that the overall brush bend continuously increases. This parameter was called ‘bend rate’ in Table 2. Fig. 5 shows a comparison of the brush deflection during the middle portion of each cycle. The trend is clear. Both brushes deflect more with more wear, but the soft brush deflects at a greater rate than the firm one. As the brush filaments bent more, the brush stiffness increased, decreasing the bend rate. This can be seen from the decreasing slope of each graph towards the end of the test.

Depth against distance at a single point of the cycle for firm and soft brushes, the soft brush deflecting faster
Fig. 5: Evolution of brush depth for firm and soft brushes at a single point in the cycle.

Conclusion

In this study, we show that the NANOVEA Tribometer can measure the depth, and thus vertical deflection, of a firm and soft toothbrush over the course of a 120 minute test. This measurement allowed for a better understanding of brush filament deflection for filaments of different stiffnesses.

The NANOVEA Tribometer could similarly be used to design tests measuring the change in stiffness of brush filaments over different temperatures, humidities, loading conditions, movement directions, trim lengths, abrasive surfaces, and other conditions. Coupled with the NANOVEA Profilometer and NANOVEA Mechanical Testers, the bend recovery and fatigue resistance of both individual filaments and the brush system as a whole could be precisely measured. NANOVEA systems can provide an invaluable source of information for all aspects of brush filament design.

The custom pin fixture allows for testing of all kinds of unique applications. NANOVEA Tribometers can be highly customized for replicating precise operating conditions, offering precise and repeatable wear and friction testing using ISO and ASTM compliant rotative and linear modes, with optional high/low temperature wear, lubrication and tribo-corrosion modules available in one pre-integrated system.

Frequently Asked Questions About Brush Bristle Testing

Why measure brush bristle stiffness?

Brushes fray with use and must be replaced. Bristles that are too stiff can wear the tooth itself rather than plaque, while bristles that are too soft lose their form faster, so the bend and wear of filaments under load guide brush design.

How can a tribometer test a toothbrush?

A toothbrush head was mounted on a 10 mm steel ball flattened on one side to make a custom pin, then run in linear reciprocating motion against an aluminum cup filled with toothpaste slurry, while the depth sensor recorded filament deflection.

What test parameters were used?

A load of 8 N, 100 rpm, a 2 mm amplitude and 120 minutes, for a total distance of 48 m (12,000 cycles), at 24 °C.

How did soft and firm brushes compare?

The soft brush’s depth changed by 0.282 mm (bend rate 7.344 × 10⁻⁴ mm/Nm) against 0.172 mm (4.479 × 10⁻⁴ mm/Nm) for the firm brush.

Is the bend rate constant?

No. The reported bend rate is an average over the test; the rate was much higher at the start and slowed as the test progressed.

What else can be studied?

Bristle stiffness at different temperatures, humidities, loads, motions, trim lengths and abrasive surfaces, and with profilometers and mechanical testers, the bend recovery and fatigue of filaments and whole brushes.

Need to Test Brushes or Filaments?