Application Note | Step Height

500nm Glass Step Height: Extreme Accuracy with Non-Contact Profilometry

Measuring a NIST-Traceable 500 nm Step Height Standard and the Noise Floor of a Chromatic Confocal Profilometer

NANOVEA profilometer and step height profile

Research & Experimental Testing

Frank Liu

Visual Design & Editorial

Andrew Shore

Introduction

Surface characterization is a current topic undergoing intense study. The surfaces of materials are important since they are the regions where physical and chemical interactions between the material and environment occur. Thus, being able to image the surface with high resolution has been desirable, since it allows scientists to visually observe the smallest surface details.

Common surface imaging data includes topography, roughness, lateral dimensions, and vertical dimensions. Identifying the load bearing surface, spacing and step height of fabricated microstructures, and defects on the surface are some applications that can be obtained from surface imaging. All surface imaging techniques, however, are not created equal.

NANOVEA’s Non-Contact Profilometry Compared to AFM Technology

With the angstrom-level vertical resolution of Atomic Force Microscopy, mapping and characterizing surface details can be done at nearly an atomic level. NANOVEA’s Profilometers are designed to reach nanometer level resolution, with many significant benefits over AFM. The non-contact optical technology of the NANOVEA system does not disturb the surface during its measurements, the ease of use minimizes sample preparation and setup time, scanning times are much shorter, and its ability to measure all types of samples are all factors that make it superior to AFMs.

With the addition of the large XY scan areas, and Z-height ranges possible, NANOVEA’s profilometers provide a system for almost any surface measurement application. With this study, we have investigated the measurement of low feature heights to showcase NANOVEA’s resolution.

ℹ️ Learn more about surface profiling lab services.

Measurement Objective

Using a NIST traceable quartz step height standard, the step height of 500nm was measured using the PS1 point sensor. The HS2000 model base was used for its zero-noise properties and air-bearing stage movement.

NANOVEA ST500 Large Area

Optical 3D Profilometer

NANOVEA ST500 large area optical profilometer for non-contact 3D surface measurement

Measurement Setup

ParameterValue
InstrumentNANOVEA HS2000, standard speed
Optical sensorPS1 lens (110 µm Z range)
Scan size3 mm x 1.5 mm
Step size0.9 µm x 4 µm
2D profile scan time (h:m:s)00:00:04
3D area scan time (h:m:s)01:03:10

Table 1: Measurement setup.

Optical pen of the profilometer above the quartz step height standard
Fig. 1: Test setup on the HS2000.

Results: Step Height

Below, the height map and a 3D view of the scanned area can be seen. The step height of 500nm, which is not discernable to the eye, is very distinct after being scanned by NANOVEA’s 3D Non-Contact Profilometer. The step height measurement of 502.4 nm matches almost exactly to 500nm etched step height. A total of 107 profiles were extracted from the area scan conducted and the step height was averaged to 502.5 ± 12.0 nm over the full 3D area scan.

Height map of the etched step region and the step analysis with plane means of 78.37 and 580.8 nm, difference 502.4 nm
Fig. 2: Height map (left) and 3D step height analysis (right).
3D view of the 500 nm step height standard showing the etched channel
Fig. 3: 3D view of the step height standard.
Overlay of 107 extracted profiles across the step with mean height 502.5 nm, standard deviation 10.95 nm
Fig. 4: Step height analysis of 107 profiles.

Noise Level

Below is a raw extracted profile from the area scans above. This is the amount of noise that is generated when measuring the quartz step height standard. Differences in height can be easily discernible if they are not hidden in the noise. The low noise observed shows that NANOVEA’s profilometer is not only limited to 500nm of height, but can measure features down to, and below 10nm.

Raw profile across the standard with noise within about plus or minus 40 nm, and its ISO 4287 amplitude parameters
Fig. 5: Raw extracted profile showing the noise level, with its ISO 4287 amplitude parameters.
ISO 4287 parameter (primary profile)Value
Pa, arithmetic mean deviation6.361 nm
Pq, root-mean-square deviation8.130 nm
Pz, maximum height63.63 nm
Pp, maximum peak height33.48 nm
Pv, maximum valley depth30.15 nm
Pt, total height63.63 nm
Pc, mean height of profile elements19.37 nm

Table 2: Noise of the raw profile (from Fig. 5).

Conclusion

The NANOVEA 3D Non-Contact Profilometer showcases its high vertical resolution abilities by scanning a step height standard of 500nm. The step height can be seen very clearly, and the obtained value of 502.5 ± 12.0 nm shows its high accuracy as well. Profiles of the scans were taken to display the amount of noise that the instrument generates. Differences in heights above the noise profile are easy to discern. This shows that while a 500nm step height was measured, higher vertical resolutions can be achieved.

Compared to other high-resolution surface metrology instruments, such as AFMs, NANOVEA’s chromatic confocal technology combined with the HS2000’s zero-noise stages provide a system with nearly angstrom-level resolution, which is superior in all other practical aspects. Therefore, unless angstrom level vertical resolution is required, NANOVEA’s Profilometers are the ideal instruments for all surface imaging due to their ease of use, fast scan times, non-contact technique, and the ability to measure all types of materials and surfaces.

Frequently Asked Questions About Nanometer Step Height Measurement

Can a non-contact profilometer measure a 500 nm step height?

Yes. A NIST-traceable 500 nm quartz step height standard measured 502.4 nm between the two planes, and 502.5 nm averaged over 107 profiles extracted from the 3D area scan.

How small a feature can it resolve?

The raw profile across the standard shows the instrument noise: Pa 6.361 nm and Pq 8.130 nm. With noise that low, the PDF concludes that features down to, and below, 10 nm can be measured.

How does chromatic confocal profilometry compare with AFM?

AFM reaches angstrom-level vertical resolution. NANOVEA profilometers reach nanometer-level resolution while measuring without contact, with minimal sample preparation, shorter scan times, large XY scan areas and Z ranges, and on all types of samples.

Why use a step height standard?

A certified, traceable step gives a known reference height, so the measured value shows the accuracy of the instrument and its noise level shows the smallest height difference it can discern.

How long does the measurement take?

A single 2D profile across the step took 4 seconds; the 3 mm x 1.5 mm 3D area scan at 0.9 µm x 4 µm steps took 1 h 3 min 10 s.

Which instrument and sensor were used?

A NANOVEA HS2000 (now succeeded by the ST500) with a PS1 point sensor (110 µm Z range), chosen for its zero-noise air-bearing stage.

Need Nanometer-Scale Height Measurements?