ABD/GLOBAL: +1-949-461-9292
AVRUPA: +39-011-3052-794
BİZE ULAŞIN

Kategori Profilometri | Pürüzlülük ve Son İşlem

 

Soft and transparent materials including a biomedical membrane, microfluidic device, and wearable sensor for non-contact profilometry applications

Non-Contact Profilometry of Soft and Transparent Materials

Application Note | Non-Contact 3D Profilometry

Non-Contact Profilometry of Soft and Transparent Materials

Comprehensive Characterization of Challenging Surfaces Without Contact, Deformation, or Sample Preparation

Examples of soft and transparent material applications for non-contact profilometry, including biomedical membranes, microfluidics, and wearable sensors

Research & Experimental Testing

Craig Leising

Visual Design & Editorial

Andrew Shore

Giriş

Soft, transparent, and easily deformable materials are increasingly important across advanced applications including flexible bioelectronics, wearable sensors, biomedical interfaces, microfluidic devices, and other polymer-based technologies. Characterizing these materials can be difficult because the measurement method itself may influence the surface or fail to capture it reliably.

Contact-based techniques can deform, scratch, or move soft materials during measurement, while transparent or absorptive surfaces can present additional challenges for some optical techniques. Non-contact profilometry avoids physical interaction with the sample while enabling quantitative surface characterization across challenging material types.

In this study, an extremely soft and translucent petroleum-jelly-based material was selected as a demanding proof-of-concept sample. Using the NANOVEA ST400 Profilometer, the surface was characterized without physical contact or sample preparation to demonstrate the broader capability of non-contact profilometry for delicate and difficult-to-measure materials.

The Advantage of Non-Contact Profilometry for Challenging Materials

Soft materials can be difficult to measure accurately because physical contact may alter the surface during the measurement itself. Films, gels, and other compliant materials can deform, scratch, or move under a contacting probe, potentially changing the geometry being characterized.

Transparent and absorptive surfaces can introduce additional measurement challenges for some optical techniques, including effects associated with light transmission, absorption, and internal reflections. NANOVEA Non-Contact Profilometers use axial chromatism to determine surface height without physically contacting the sample.

This combination enables quantitative characterization of challenging surfaces while minimizing measurement influence. Depending on the application, measurements can include surface roughness, flatness, 3D topography, surface area, profile geometry, and other dimensional characteristics without requiring sample preparation.

Ölçüm Hedefi

The objective of this study was to demonstrate non-contact surface characterization on an extremely soft and translucent material, representing the type of measurement challenge encountered when a surface may be altered by physical contact or prove difficult for some optical techniques.

A petroleum-jelly-based lip balm was selected as a deliberately challenging proof-of-concept sample because of its softness and translucency. The sample was measured using the NANOVEA ST400 Profilometer without physical contact or sample preparation.

The resulting measurement was used to obtain 3D topography, 2D profile data, surface roughness, flatness, and 3D surface area, demonstrating the range of quantitative surface information that can be obtained from a delicate material using non-contact profilometry.

NANOVEA ST400 Non-Contact

Optik Profilometre

Optical Profilometry Results

Soft transparent petroleum-jelly-based lip balm sample used for non-contact profilometry

Soft, translucent petroleum-jelly-based sample used for non-contact profilometry.

Soft transparent petroleum-jelly-based sample positioned under the NANOVEA ST400 profilometer for non-contact surface measurement

The sample being scanned by the NANOVEA ST400 for non-contact surface measurement.

3D Profile Measurement

The NANOVEA ST400 captured the 3D surface of the extremely soft and translucent sample without physically contacting the material. The resulting topography was used to evaluate multiple aspects of the surface, including ISO 25178 surface parameters, 3D surface area, and flatness corresponding to ISO 12781. A 2D cross-section was also extracted from the measurement to provide additional profile detail.

Obtaining these measurements from such a soft and translucent surface demonstrates the value of non-contact profilometry for materials that could otherwise be altered by a contacting probe or present challenges for some optical techniques. Quantitative surface geometry can be acquired while preserving the condition of the measured surface.

3D non-contact profilometry measurement of a soft transparent petroleum-jelly-based sample with ISO 25178 surface parameters

3D surface profile of the soft, transparent sample with ISO 25178 surface parameters and flatness analysis.

2D Profile Measurement

2D profile extracted from non-contact profilometry of a soft transparent petroleum-jelly-based sample

2D profile extracted from the non-contact 3D surface measurement across a 4 mm section of the sample.

An intensity/contrast image was also acquired simultaneously with the 3D surface measurement, providing complementary visual information alongside the measured topography.

False-color height map from non-contact profilometry of a soft transparent petroleum-jelly-based sample

False-color height map showing surface height variation across the soft, translucent sample.

Intensity image acquired during non-contact profilometry of a soft transparent petroleum-jelly-based sample

Intensity image acquired simultaneously with the 3D surface measurement.

Sonuç

This study demonstrates how non-contact profilometry can characterize surfaces that combine two particularly difficult measurement conditions: extreme softness and translucency. Using the NANOVEA ST400, quantitative 3D surface data were acquired without physically contacting or preparing the sample.

A petroleum-jelly-based lip balm was selected as a deliberately challenging proof-of-concept material rather than as the end application itself. Its soft, translucent surface provided a practical demonstration of the ability to obtain surface roughness, flatness, 3D surface area, profile geometry, and complementary intensity data while minimizing the influence of the measurement process on the surface.

This capability is relevant wherever delicate, compliant, transparent, or absorptive materials must be characterized without deformation or surface damage. As soft polymers, gels, transparent elastomers, and related materials continue to appear in areas such as biomedical interfaces, wearable technologies, microfluidics, and advanced polymer systems, non-contact surface measurement provides a useful approach for evaluating their surface geometry and topography.

Frequently Asked Questions About Non-Contact Profilometry

Why is non-contact profilometry useful for soft materials?

Soft materials can deform, scratch, or move when touched by a contacting probe. Non-contact profilometry measures the surface optically, reducing the risk that the measurement itself alters the geometry being characterized.

Can non-contact profilometry measure transparent materials?

Yes, depending on the optical technology and material. NANOVEA profilometers use axial chromatism to determine surface height and can characterize transparent, opaque, specular, diffusive, polished, and rough surfaces without physical contact.

Can soft and transparent surfaces be measured without sample preparation?

In this study, the soft and transparent petroleum-jelly-based sample was measured without sample preparation. Avoiding coatings or other surface modification can be especially valuable when the original surface condition needs to be preserved.

What can be measured with non-contact 3D profilometry?

Non-contact 3D profilometry can provide quantitative measurements including surface roughness, 3D topography, flatness, surface area, 2D profiles, and other dimensional characteristics, depending on the measurement objective and surface geometry.

What types of materials benefit from non-contact surface measurement?

Non-contact measurement is especially useful for materials that are soft, delicate, transparent, semi-transparent, easily scratched, or otherwise difficult to probe physically. It can also be useful when maintaining the original surface condition is important.

How is non-contact profilometry different from contact profilometry?

Contact profilometry uses a physical stylus that moves across the surface. Non-contact profilometry acquires surface height optically, eliminating probe-to-sample contact and reducing the possibility of contact-induced deformation, scratching, or movement on sensitive materials.

Pacemaker and endocardial pacing leads shown in a translucent medical illustration for pacing lead insulation wear testing

Pacing Lead Insulation Wear Testing in Hanks’ Solution

Application Note | Medical Device Tribology

Nano-Friction and Wear Testing of Pacing Lead Insulation in Hanks’ Solution

Tribological analysis of silicone and polyether-polyurethane endocardial lead materials

Medical illustration of a pacemaker with two endocardial pacing leads routed into the heart for pacing lead insulation wear testing context

Research & Experimental Testing

Duanjie Li, PhD

Visual Design & Editorial

Andrew Shore

Giriş

A pacemaker is a medical device used to regulate heart rhythm and maintain an adequate heart rate. It is typically implanted in the chest or abdomen and sends electrical impulses to the heart muscle through endocardial pacing leads.

As pacemakers remain a widely used treatment for cardiac rhythm disorders, the quality and service life of pacing leads are critical to long-term device performance. Lead failures can create serious risks for patients and may require surgical replacement, making pacing lead insulation wear testing an important part of material evaluation for implantable cardiac devices.1–5
Endocardial pacing leads with insulated lead bodies used in implantable cardiac devices

Endocardial pacing leads transmit electrical impulses from a pacemaker to the heart while operating in a dynamic body-fluid environment.

Why Friction and Wear Matter for Endocardial Lead Insulation

The outer insulation material of an endocardial lead requires several key properties, including biological inertness, high flexibility, fracture toughness, and long service life. Low friction can reduce interaction between the lead and the blood vessel, helping minimize vessel irritation during implantation and movement.

Wear resistance is also critical. Endocardial leads experience continuous movement from the heart and surrounding body structures, while operating in a body-fluid environment that can influence friction, wear, and material response.

Because of this complex environment, endocardial lead insulation should be evaluated using controlled tribological methods that simulate relevant contact conditions. Testing in Hanks’ solution allows the friction and wear behavior of lead insulation materials to be compared under a simulated body-fluid condition rather than relying only on dry testing.

Nano-friction test setup for measuring pacing lead insulation materials in Hanks’ solution

Nano-friction test setup used to evaluate endocardial pacing lead insulation materials under low-load contact conditions.

Ölçüm Hedefi

This study compares the nano-friction and wear behavior of endocardial pacing lead insulation materials in Hanks’ solution. Silicone and polyether-polyurethane lead materials were evaluated to determine how each material responds under simulated body-fluid conditions.

Low-load nano-friction testing was performed using the Nano Module of the NANOVEA Mekanik Test Cihazı to measure coefficient of friction at controlled contact force. Reciprocating wear testing was then performed using a NANOVEA Tribometer to compare wear resistance under linear sliding contact.

NANOVEA T50 Kompakt
Serbest Ağırlık Tribometresi

NANOVEA PB1000 Büyük Platform Mekanik Test Cihazı

Measurement Principle

Nano-Friction Measurement Principle

Nano-friction testing measures the coefficient of friction (COF) between the test surface and a controlled counter material under very low applied load. In this study, the indenter made contact with the pacing lead insulation surface while the Nano Module maintained a constant load throughout the measurement.

The Nano Module uses a fast piezoelectric system and load cell to adjust the ball position and keep the applied load stable during sliding. The sample is moved at a controlled speed while lateral force is measured and plotted against displacement.

A stainless steel ball with a 6 mm diameter is commonly used for this type of measurement, although other counter materials, shapes, and sizes can be selected to simulate different contact conditions. This allows pacing lead insulation materials to be evaluated under controlled low-load friction conditions relevant to biomedical device applications.

Schematic of the nano-friction measurement principle showing a ball-tip indenter under controlled constant load, a capacitive depth sensor, non-destructive load, and reciprocating sample motion on a friction spring table

Nano-friction measurement schematic showing controlled low-load sliding contact and lateral force measurement during reciprocating motion.

Reciprocating Wear Principle

Reciprocating wear testing evaluates material response under repeated linear sliding contact. A flat or spherical counter material is loaded against the test sample with a precisely known force, while the sample moves back and forth in a controlled reciprocating motion.

The counter material, such as a pin or ball, is mounted on a stiff lever that functions as a low-friction force transducer. As the sample moves, frictional forces between the counter material and the sample are measured using a strain gauge sensor on the tribometer arm.

After the test, the resulting wear track can be examined to compare material damage, wear scar geometry, and surface response. This method allows friction and wear behavior to be studied under controlled conditions, including variations in time, contact pressure, sliding speed, temperature, humidity, and lubrication environment.

Schematic of the reciprocating wear principle showing adjustable weights, tribometer arm, pin or ball holder, strain gauge, sample stage, linear wear track, and linear reciprocating motion

Linear reciprocating wear schematic showing a pin or ball counterface sliding across the sample to generate a wear track under controlled load.

Test Prosedürü

The coefficient of friction (COF) of the pacing lead materials was measured against a stainless steel 440 ball with a 6 mm diameter. Testing was performed using the Nano Module of the Nanovea Mechanical Tester.

The sample was immersed in Hanks’ solution to simulate a body-fluid environment. A low applied load of 50 mN was maintained throughout the test, while the ball slid against the lead surface at a constant speed of 20 mm/min over a total sliding distance of 10 mm.

Wear resistance was evaluated using a Nanovea Tribometer with the Linear Reciprocating Wear Module. During the wear test, a stainless steel 303 block measuring 10 × 10 mm² was used as the counter material, and the coefficient of friction was recorded in situ at 0.1 s intervals.

After testing, the resulting wear tracks were examined under an optical microscope to compare surface damage on the silicone and polyether-polyurethane lead materials. Stainless steel was used as the counter material in this study; however, custom fixtures and alternative counter materials can be used to simulate specific application conditions.

Parameter Value
Sample Leads made of silicone or polyether-polyurethane (PP)
Normal force 1 N
Hız 200 cycles/min
Duration of test 5 h
Çevre Hanks’ solution

Wear test parameters used to evaluate silicone and polyether-polyurethane pacing lead materials in Hanks’ solution.

Sonuçlar ve Tartışma

Nano-Friction Test

The nano-friction behavior of the silicone and polyether-polyurethane (PP) pacing lead materials was first evaluated using the Nano Module of the Nanovea Mechanical Tester. The coefficient of friction was measured in both dry conditions and Hanks’ solution to compare material response under ambient and simulated body-fluid environments.

Both materials showed significantly lower coefficient of friction in Hanks’ solution than under dry conditions. In Hanks’ solution, the silicone lead exhibited a COF of approximately 0.15, while the polyether-polyurethane lead exhibited a lower COF of approximately 0.05. Under dry conditions, the values were substantially higher, at approximately 0.6 for silicone and 0.5 for polyether-polyurethane.

These results demonstrate the importance of testing pacing lead insulation materials under application-relevant environmental conditions. Hanks’ solution had a strong effect on the measured friction behavior, showing that dry testing alone may not represent the tribological response of lead insulation materials in a simulated body-fluid environment.

The low-load control of the Nano Module allowed the applied force to remain constant at 50 mN during the measurement. This enabled controlled simulation of low-contact-force interaction between the lead material and surrounding biological structures.

Graph comparing coefficient of friction of silicone and polyether-polyurethane pacing lead materials in dry conditions and Hanks’ solution

Coefficient of friction comparison for silicone and polyether-polyurethane pacing lead materials in dry conditions and Hanks’ solution.

Wear Test

Wear resistance was evaluated using a Nanovea Tribometer to compare the silicone and polyether-polyurethane pacing lead materials in Hanks’ solution. After testing, the lead surfaces were examined visually and under optical microscopy to compare the extent of wear damage.

The silicone lead showed a large wear scar with a width of approximately 1.2 mm. Microscopic observation indicated severe wear on the silicone lead, with parallel deep grooves formed along the movement direction of the rubbing block.

In comparison, the polyether-polyurethane lead showed a narrower wear scar of approximately 0.6 mm. The observed wear was milder, with only several small scratches visible on the shallow surface.

Wear of the lead outer insulation can contribute to pacing and sensing abnormalities, making wear resistance an important factor in endocardial lead material selection.6 These results indicate that polyether-polyurethane provided lower friction and better wear resistance than silicone under the tested conditions.

Before-and-after wear comparison of silicone and polyether-polyurethane pacing lead surfaces, including 400x microscope images showing more severe wear on silicone and milder wear on polyether-polyurethane.

Silicone pacing lead surface before wear testing in Hanks’ solution

Silicone pacing lead surface before reciprocating wear testing.

Polyether-polyurethane pacing lead surface before wear testing in Hanks’ solution

Polyether-polyurethane pacing lead surface before reciprocating wear testing.

Silicone pacing lead surface after wear testing showing a large wear scar

Silicone pacing lead surface after wear testing, showing a pronounced wear scar.

Polyether-polyurethane pacing lead surface after wear testing showing a smaller wear scar

Polyether-polyurethane pacing lead surface after reciprocating wear testing.

Microscope image at 400x magnification showing severe wear grooves on silicone pacing lead surface

400x microscope image of the silicone pacing lead after wear testing, showing deep parallel wear grooves.

Microscope image at 400x magnification showing mild wear on polyether-polyurethane pacing lead surface

400x microscope image of the polyether-polyurethane pacing lead after wear testing, showing comparatively mild surface wear.

Sonuç

This study demonstrated the use of low-load nano-friction testing and reciprocating wear testing to evaluate endocardial pacing lead insulation materials in Hanks’ solution. The Nano Module of the NANOVEA Mechanical Tester measured coefficient of friction under controlled low-load contact, while the NANOVEA Tribometer simulated wear behavior under reciprocating sliding motion.

Testing in Hanks’ solution showed a clear difference between silicone and polyether-polyurethane lead materials. Polyether-polyurethane exhibited lower coefficient of friction and better wear resistance than silicone under the tested conditions, making it the stronger candidate for the outer insulation material of endocardial pacing leads in this study.

These results highlight the importance of evaluating biomedical materials under application-relevant environments rather than relying only on dry testing. Controlled nano-friction and tribology testing can help compare candidate materials, quantify friction response, and evaluate wear resistance for implantable medical device components.

The NANOVEA Mechanical Tester’s Nano, Micro, and Macro modules operate within a single ISO and ASTM compliant platform, enabling consistent evaluation of hardness, elastic modulus, fracture toughness, and wear from a single system. The NANOVEA Tribometer similarly supports rotative and linear wear modes with optional high-temperature, corrosion, and liquid environment modules.

Referanslar

[1] Magney JE, Flynn DM, Parsons JA, Staplin DH, Chin-Purcell MV, Milstein S, Hunter DW. Pacing Clin Electrophysiol. 1993; 16:445–457.
[2] Jacobs DM, Fink AS, Miller RP, Anderson WR, McVenes RD, Lessar JF, Cobian KE, et al. Pacing Clin Electrophysiol. 1993; 16:434–444.
[3] Gupta K, Villareal RP, Rasekh A, Massumi A. Tex Heart Inst J. 2003; 30:84–85.
[4] Magney JE, Parsons JA, Flynn DM, Hunter DW. Pacing Clin Electrophysiol. 1995; 18:1509–1517.
[5] Kazama S, Nishiyama K, Machii M, Tanaka K, Amano T, Nomura T, Ohuchi M, et al. Jpn Heart J. 1993; 34:193–200.
[6] Andrzej K, Barbara M, Agnieszka K, Marcin G. Pacing Clin Electrophysiol. 2013; 36(12):1503–1511.

Frequently Asked Questions About Pacing Lead Insulation Wear Testing

How do you evaluate friction and wear behavior of pacing lead insulation?

Pacing lead insulation can be evaluated using low-load friction testing and reciprocating wear testing. These methods measure coefficient of friction, wear scar formation, and surface damage under controlled load, motion, and environmental conditions.

Why is low-load friction testing important for endocardial leads?

Endocardial leads operate under relatively low contact forces while interacting with blood vessels, tissue, and surrounding structures. Low-load friction testing helps evaluate how insulation materials behave under contact conditions that are closer to the application than high-force mechanical testing alone.

What does coefficient of friction indicate in pacing lead material testing?

Coefficient of friction indicates how much resistance occurs during sliding contact between the lead insulation and a counter material. In this study, lower COF values in Hanks’ solution showed that the test environment had a strong effect on the measured friction behavior of silicone and polyether-polyurethane materials.

Why compare silicone and polyether-polyurethane lead insulation materials?

Silicone and polyether-polyurethane are commonly considered for flexible biomedical insulation applications because they can provide different combinations of flexibility, durability, and surface response. Comparing them under the same test conditions helps identify which material provides lower friction and better wear resistance for the intended application.

Which NANOVEA instruments are used for low-load friction and wear testing?

Low-load coefficient of friction can be measured using the Nano Module of a NANOVEA Mechanical Tester, while reciprocating wear behavior can be evaluated using a NANOVEA Tribometer. Together, these systems allow controlled evaluation of friction, wear, and material response for biomedical components.

How is reciprocating wear testing used for pacing lead materials?

Reciprocating wear testing repeatedly slides a counter material across the sample surface under controlled load to create and evaluate a wear track. For pacing lead insulation materials, this allows comparison of wear scar width, surface damage, and material durability under simulated sliding contact.

Need Reliable Medical Device Friction and Wear Testing?

3D optical profilometry image showing climbing hold surface roughness, pore morphology, and grip-related texture features.

Climbing Hold Surface Roughness Analysis

Application Note | 3D Optical Profilometry

Climbing Hold Surface Roughness Analysis Using 3D Optical Profilometry

Measuring Texture, Porosity, and Topography on Bouldering Holds

Bouldering holds analyzed for climbing hold surface roughness using 3D optical profilometry.

Research & Experimental Testing

Walter Alabiso, PhD

Visual Design & Editorial

Andrew Shore

Giriş

Bouldering is a demanding discipline that combines physical strength, precise body positioning, and an understanding of how the human body interacts with climbing surfaces. On slab routes, where the wall is angled below vertical and positive holds are limited or absent, a climber’s stability depends almost entirely on the tribological interaction between the body and the climbing hold surface.

Climbing hold surface roughness plays a central role in this contact. Roughness provides the microtexture needed for smearing, a technique where high-friction rubber soles are pressed firmly against the surface to expand the effective contact area and generate adherence. A similar mechanism occurs at the fingers, where the ridges of fingerprints and the pliability of skin deform slightly against the hold’s surface features, creating grip through microscopic interlocking.

Porosity contributes to grip performance by absorbing moisture, sweat, or chalk at the contact interface, preventing the formation of a thin lubricating film that would reduce friction. Micro-cracks and surface flaws act as additional friction points, helping the climber maintain lateral tension against the hold surface. Because these features (roughness, porosity, and surface morphology) operate at different scales and interact differently depending on the hold, quantitative 3D surface measurement is essential for comparing how different climbing hold textures perform under real contact conditions.

Bouldering grips used to compare surface roughness, pore morphology, and grip-related topography.

Why Use Non-Contact Profilometry for Climbing Hold Surface Analysis

Climbing holds and rock-like surfaces can include deep pores, steep asperities, sharp valleys, and irregular texture. These features are difficult to measure accurately with contact-based profilometry because a physical stylus can lose contact, deform local surface features, or fail to reach narrow cavities.

NANOVEA’s non-contact optical profilometry uses chromatic light technology to capture surface height data without touching the sample. This makes it suitable for reconstructing complex climbing hold topography, including deep nooks, pores, and surface flaws, while avoiding measurement artifacts caused by local plastic deformation.

Ölçüm Hedefi

The objective of this study was to demonstrate how non-contact 3D optical profilometry can be used to reconstruct and compare the surface roughness, topography, and pore morphology of climbing holds.

Two bouldering grip samples were analyzed: a yellow hold with a smoother, flatter surface and a blue hold with a rougher tactile texture and sharper grip features. The analysis focused on surface height variation, areal roughness parameters, pore coverage, pore size, pore depth, and functional surface behavior.

The NANOVEA JR25 Optical Profilometer measuring the climbing hold samples using an optical sensor.

Measurement Method

Bu NANOVEA JR25 Optical Profiler was used to measure the yellow and blue bouldering grip samples. Each surface was scanned with a PS4-MG35 single-point optical sensor with an enhanced 3000 µm Z-range, allowing the system to capture deep pores, sharp valleys, and irregular surface texture while maintaining a 4 µm acquisition step in X and Y.

Dual-frequency acquisition was used to reduce light sensor saturation from localized bright spots on the grip surfaces, improving data capture across rough, porous, and uneven areas.

NANOVEA JR25 Portable

Optik Profilometre

Test Parametreleri

Measurement Setting Optical Profilometry Setup
Samples measured Yellow and blue bouldering grip samples
Optical pen PS4-MG35
Z-range 3000 µm
Scan area 5.00 mm × 5.00 mm
X-step size 4.00 µm
Y-step size 4.00 µm
Averaging 1
Measurement type Direct
Acquisition mode Dual frequency
Acquisition rate 100–400 Hz
Light intensity 100%

Optical profilometry test conditions used to measure the bouldering grip samples.

Optical Profilometry Results

Yellow Grip Sample

Surface Roughness Analysis

The 3D rendering below shows the reconstructed surface topography of the yellow climbing grip sample.

3D optical profilometry reconstruction of the yellow climbing grip surface showing pores, roughness, and surface height variation.

A total least-squares plane was removed to study surface properties. The roughness filters S-Gaussian 2.5 µm was applied following ISO 25178 (1/2 cut-off removed at each side). However, the sharp density of pores and asperities and the elevated average roughness make the use of a Gaussian L-filter (8 mm cut off) inapplicable. Therefore, the primary surface was considered, and the roughness parameters are listed in the table below, alongside the 2D false-color map of the filtered surface.

False-color optical profilometry surface roughness map of the yellow climbing grip sample with ISO 25178 height parameters.
ISO 25178-2 – Primary Surface
S-filter (λs): Gaussian, 2.5 µm, 1/2 cut-off
F-operation: [Workflow] Leveled (TLSPL)
Height Parameters
Sq 168.970 µm Kök ortalama kare yüksekliği
Ssk -0.927 Çarpıklık
Sku 4.117 Kurtosis
Sp 320.530 µm Maksimum tepe yüksekliği
Sv 868.116 µm Maximum pit depth
Sz 1188.645 µm Maksimum yükseklik
Sa 132.953 µm Aritmetik ortalama yükseklik

The average surface roughness Sa is 132.953 µm, whereas the peak-to-valley roughness, Sz amounts to 1188.645 µm. The surface morphology is skewed towards deep valleys (Ssk < 0, Sv > Sp), with a leptokurtotic (Sku > 3) distribution of peaks and valleys relative to the average plane.

The following picture shows a 2D photo-simulation of the area under artificial lighting, highlighting the region’s morphology.

2D photo simulation of the yellow climbing grip surface showing pores, roughness, and morphology under artificial lighting.

Pore Morphology Analysis

A pore analysis was performed across the full scanned area using a semi-automated edge-detection algorithm. The analysis identified recessed surface features to quantify pore coverage, pore density, radius, void volume, and maximum depth.

Pore detection analysis of the yellow climbing grip surface using semi-automated edge detection to identify recessed surface features.

The detected pore locations were then mapped across the scanned 5 mm × 5 mm area to evaluate pore coverage, density, and size distribution.

Pore distribution map of the yellow climbing grip sample showing detected recessed surface features across a 5 mm by 5 mm scanned area.
Information
MethodCircle detection
Features detectedPores, recessed objects
Minimum detection diameter0.150 mm
Maximum detection diameter2.000 mm
Number of detected pores206
Surface coverage47.395%
Pore density8.203 particles/mm²
Global Statistics
ParameterUnitMeanStd. Dev.MinMax
Yarıçapmm0.1270.0490.0760.275
Void volumeµm³4,724,770.7056,748,143.92523,594.1724.422 × 10⁷
Maximum depthµm173.72994.94228.153716.480

Pores covered nearly half of the yellow grip’s scanned surface, with a measured coverage of 47.395% and a pore density of 8.203 particles/mm². The detected pores and cracks were highly heterogeneous in size, volume, and depth, ranging from large crater-like features with a maximum radius of 0.275 mm and void volume above 4.4 × 10⁷ µm³ to smaller pores with a minimum radius of 0.076 mm and void volume of 23,594.172 µm³. This uneven pore distribution is reflected in the large standard deviation measured for void volume and maximum depth.

Functional Surface Parameters (Abbott-Firestone curve)

The Abbott-Firestone curve shows the cumulative areal material distribution of the yellow climbing grip sample. This analysis defines functional surface parameters including Sk, Spk, and Svk according to ISO 25178-2.

Abbott-Firestone curve for the yellow climbing grip sample showing cumulative areal material distribution and functional surface parameters.
Information
Standart ISO 25178-2
Parameter Value Unit
Sk 409.738 µm
Spk 45.480 µm
Svk 233.446 µm
Smrk1 3.976 %
Smrk2 85.005 %

The chart below shows the peak-valley distribution from the mean plane based on the functional parameters derived from the Abbott-Firestone curve. Valleys are shown in purple, the mean plane in green, and peaks in orange.

Peak-valley distribution map of the yellow climbing grip sample showing valleys, mean plane regions, and peaks derived from Abbott-Firestone functional parameters.
Information
1st threshold Height – c1: 229.209 µm
2nd threshold Height – c2: -180.424 µm
Parameters Unit
Projected area (in %) % 14.995 81.029 3.976
Projected area mm² 3.772 20.381 1.000
Volume of material (in %) % 97.451 48.100 0.973
Volume of material µm³ 1.684 × 10¹⁰ 4.956 × 10⁹ 2.275 × 10⁷

The yellow grip sample shows a dominant mean-plane region with scattered recessed pores and a smaller population of raised peaks. This indicates a surface texture characterized mainly by average-sized pores distributed across the scanned area.

Blue Grip Sample

Surface Roughness Analysis

The 3D rendering below shows the reconstructed surface topography of the blue climbing grip sample.

3D optical profilometry reconstruction of the blue climbing grip surface showing roughness, pores, asperities, and surface height variation.

A total least-squares plane was removed to evaluate the blue grip’s surface properties. An S-Gaussian 2.5 µm roughness filter was applied following ISO 25178, with 1/2 cut-off removed at each side.

Because of the dense pores, asperities, and elevated average roughness, a Gaussian L-filter with an 8 mm cut-off was not applied. The primary surface was used for roughness analysis, with the roughness parameters listed alongside the 2D false-color map of the filtered surface.

False-color optical profilometry surface roughness map of the blue climbing grip sample with ISO 25178 height parameters.
ISO 25178-2 – Primary Surface
S-filter (λs): Gaussian, 2.5 µm, 1/2 cut-off
F-operation: [Workflow] Leveled (TLSPL)
Height Parameters
Sq 211.440 µm Kök ortalama kare yüksekliği
Ssk -0.682 Çarpıklık
Sku 3.672 Kurtosis
Sp 522.404 µm Maksimum tepe yüksekliği
Sv 720.164 µm Maximum pit depth
Sz 1242.568 µm Maksimum yükseklik
Sa 166.719 µm Aritmetik ortalama yükseklik

The blue grip sample had an average surface roughness, Sa, of 166.719 µm and a peak-to-valley roughness, Sz, of 1242.568 µm. The negative skewness value, Ssk &lt; 0, indicates that the surface morphology is skewed toward deep valleys, while Sv &gt; Sp shows that the maximum pit depth exceeded the maximum peak height.

The kurtosis value, Sku &gt; 3, indicates a leptokurtotic height distribution, meaning the blue grip surface contains sharper or more extreme peaks and valleys relative to the average plane.

The 2D photo simulation below highlights the blue climbing grip’s surface morphology under artificial lighting.

2D photo simulation of the blue climbing grip surface showing pores, roughness, and morphology under artificial lighting.

Pore Morphology Analysis

A pore analysis was performed across the full scanned area using a semi-automated edge-detection algorithm. The analysis identified recessed surface features to quantify pore coverage, pore density, radius, void volume, and maximum depth.

Pore detection analysis of the blue climbing grip surface using semi-automated edge detection to identify recessed surface features.

The detected pore locations were mapped across the scanned 5 mm × 5 mm area to evaluate pore coverage, density, and size distribution.

Pore distribution map of the blue climbing grip sample showing detected recessed surface features across a 5 mm by 5 mm scanned area.
Information
Method Circle detection
Features detected Pores, recessed objects
Minimum detection diameter 0.040 mm
Maximum detection diameter 2.000 mm
Number of detected pores 794
Surface coverage 24.208%
Pore density 31.355 particles/mm²
Global Statistics
Parameter Unit Mean Std. Dev. Min Max
Yarıçap mm 0.035 0.035 0.020 0.218
Void volume µm³ 821,872.849 2,495,310.021 11,009.819 2.929 × 10⁷
Maximum depth µm 476.053 305.830 16.132 1044.045

Pores covered 24.208% of the blue grip’s scanned surface, with a pore density of 31.355 particles/mm². The detected pores and cracks were highly heterogeneous in size, volume, and depth, ranging from large crater-like features with a maximum radius of 0.218 mm and void volume greater than 2.9 × 10⁷ µm³ to small pores with a minimum radius of 0.020 mm and void volume of approximately 1.1 × 10⁴ µm³.

This uneven distribution is reflected in the large standard deviation measured for void volume and maximum depth. The pore distribution is bimodal, with one population of fine, deep pores and another population of larger crater-like valleys.

Functional Surface Parameters (Abbott-Firestone curve)

The Abbott-Firestone curve shows the cumulative areal material distribution of the blue climbing grip sample. This analysis defines functional surface parameters including Sk, Spk, and Svk according to ISO 25178-2.

Abbott-Firestone curve for the blue climbing grip sample showing cumulative areal material distribution and functional surface parameters.
Information
Standart ISO 25178-2
Parameter Value Unit
Sk 522.359 µm
Spk 117.670 µm
Svk 295.209 µm
Smrk1 6.122 %
Smrk2 87.456 %

The chart below shows the peak-valley distribution from the mean plane based on the functional parameters derived from the Abbott-Firestone curve. Valleys are shown in purple, the mean plane in green, and peaks in orange.

Peak-valley distribution map of the blue climbing grip sample showing valleys, mean-plane regions, and peaks derived from Abbott-Firestone functional parameters.
Information
1st threshold Height – c1: 283.646 µm
2nd threshold Height – c2: -238.619 µm
Parameters Unit
Projected area (in %) % 12.544 81.334 6.122
Projected area mm² 3.182 20.629 1.553
Volume of material (in %) % 96.079 48.546 1.514
Volume of material µm³ 1.151 × 10¹⁰ 6.431 × 10⁹ 9.142 × 10⁷

The blue grip sample shows a dominant mean-plane region with fine, deep pores distributed across the surface and localized peak features. Compared with the yellow grip, the blue grip contains a higher projected peak area and a bimodal pore structure, combining fine recessed pores with larger crater-like valleys.

Sonuç

In this application, the NANOVEA JR25 Non-Contact Optical Profiler was used to measure the surface roughness, topography, and pore morphology of yellow and blue bouldering grip samples.

Topographic analysis showed that both grip samples had high surface roughness, with Sa values above 100 µm and Sz values above 1000 µm. Both surfaces also showed an asymmetric height distribution skewed toward valleys, indicating that recessed features played a major role in the measured surface morphology.

The yellow grip sample showed higher pore coverage, with pores covering 47.395% of the scanned surface. Its surface was mainly characterized by average-sized pores distributed across the measured area.

The blue grip sample showed lower pore coverage at 24.208%, but a much higher pore density of 31.355 particles/mm². Its pore distribution was bimodal, with a population of fine, deep pores and a separate population of larger crater-like valleys.

These results show how non-contact 3D optical profilometry can quantify climbing hold surface features that are difficult to evaluate from visual inspection alone, including roughness, pore coverage, pore depth, surface height distribution, and functional topography. The blue grip’s higher porosity and bimodal pore structure make it more likely to absorb moisture and chalk at the contact interface, while its elevated roughness and surface morphology support stable friction for shoe rubber and finger contact. The yellow grip’s lower roughness and flatter profile suggest it is better suited for use as a foothold in slab climbing, where broad surface contact matters more than deep textural engagement.

Frequently Asked Questions About Climbing Hold Surface Roughness

What is climbing hold surface roughness?

Climbing hold surface roughness describes the height variation, texture, pores, asperities, and valleys present on the surface of a climbing grip. These features can influence contact behavior between the hold, shoe rubber, skin, chalk, and moisture.

How can climbing hold surface roughness be measured?

Climbing hold surface roughness can be measured using non-contact 3D optical profilometry. This method reconstructs the surface topography and calculates areal roughness parameters such as Sa, Sz, Sp, Sv, Ssk, and Sku without touching or deforming the sample.

Why use non-contact optical profilometry for climbing hold analysis?

Non-contact optical profilometry is useful for climbing hold analysis because climbing grips can contain deep pores, sharp valleys, rough asperities, and irregular surface texture. A contact stylus may lose contact, fail to reach recessed features, or introduce artifacts on complex surfaces.

What does Sa mean in surface roughness analysis?

Sa is the arithmetic mean height of a surface and is commonly used to describe average areal surface roughness. In this app note, both climbing grip samples showed high Sa values above 100 µm, indicating strongly textured surfaces.

What does Sz mean in optical profilometry results?

Sz is the maximum height of the measured surface, calculated from the highest peak to the deepest valley. In climbing hold surface roughness analysis, Sz helps describe the full vertical range of the grip’s surface texture.

Why is pore morphology important for climbing grips?

Pore morphology can affect how a climbing grip interacts with chalk, sweat, humidity, skin, and shoe rubber. Measuring pore coverage, density, depth, and volume helps quantify surface features that are difficult to evaluate by visual inspection alone.

stent coating adhesion testing failure analysis drug eluting stent coating

Stent Coating Adhesion and Delamination Analysis Using Nano Scratch Testing

Application Note | Stent Coating Adhesion Testing

Stent Coating Adhesion and Delamination Analysis Using Nano Scratch Testing

Quantifying Coating Failure and Adhesion Performance on Drug-Eluting Stents

stent coating adhesion testing nano scratch delamination critical load

Research & Experimental Testing

Duanjie Li, PhD

Visual Design & Editorial

Andrew Shore

Giriş

Blood is carried through arteries from the heart to the rest of the body. Any weakening or blockage of these vessels can pose significant health risks and may become life-threatening. A stent is a small mesh tube inserted into the lumen of a blood vessel to treat narrowed or weakened arteries. Stent implantation is now a widely used procedure to support the arterial wall and restore blood flowᶦ.

Metal stent mesh geometry illustrating the structural complexity of vascular implant design.

Why coating adhesion matters in drug-eluting stents

Drug-eluting stents represent a major advancement in stent technology. They incorporate a biodegradable, biocompatible polymer coating that enables controlled drug release at the arterial site, helping to inhibit intimal thickening and reduce the risk of restenosisᶦᶦ.

A critical concern in these systems is the delamination of the polymer coating from the metallic stent substrate. This coating carries the drug-eluting layer, and its adhesion directly impacts device performance and reliability.

To improve coating adhesion, stents are often designed with complex geometries. In this study, the polymer coating is located at the bottom of grooves within the stent mesh. This configuration presents a significant challenge for adhesion measurement.

A reliable method is required to quantitatively evaluate the interfacial strength between the polymer coating and the metal substrate. The small diameter of the stent mesh, comparable to a human hair, combined with its three-dimensional geometry, requires:

  • ultrafine X-Y positioning accuracy
  • precise control of applied load
  • accurate depth measurement during testing

Measurement Method

Nano scratch testing is performed using the NANOVEA PB1000 Mekanik Test Cihazı, in Nano Scratch Mode, to evaluate the cohesive and adhesive strength of the polymer coating on the metal mesh of stent samples.

Controlled scratch measurements are carried out on stent geometries with dimensions comparable to a human hair, enabling precise evaluation of coating adhesion on complex stent structures.

NANOVEA PB1000 Advanced

Mekanik Test Cihazı

Test Koşulları

1. Regular Stent Samples

The stent is fixed on the sample stage, with a support wire inserted inside the stent tube to ensure stability during nano scratch testing. The NANOVEA Mechanical Tester is used to perform nano scratch measurements using the parameters summarized in Table 1, to evaluate the cohesive and adhesive strength of the polymer coating on the metal substrate.

ParameterValue
Load typeİlerici
Initial load0.05 mN
Final load300 and 100 mN
Sliding speed0.5 mm/min
Sliding distance0.5 mm
Indenter geometryKonik
Indenter material (tip)Elmas
Girinti ucu yarıçapı20 µm
Sıcaklık24°C (room)

Tablo 1: Test parameters for nano scratch measurements on regular stent samples

2. Grooved Stent Samples

The SEM image in Fig. 1 shows the cross-section of the stent sample. The stent features a groove with a depth of approximately 30 µm. The polymer coating, with a thickness of 10.8 µm, is located at the bottom of the groove.

Standard 60° conical diamond tips are not sharp enough to reach the bottom of the groove without contacting the sidewalls. Therefore, a sharper 40° conical diamond tip is used in this study (Fig. 2).

Nano scratch measurements are performed using the parameters summarized in Table 2.

Parameter Value
Load type İlerici
Initial load 0.1 mN
Final load 300 mN
Yükleme oranı 300 mN/min
Scratch length 0.25 mm
Scratch speed 0.25 mm/min
Indenter geometry 40° cone
Indenter material (tip) Elmas
Girinti ucu yarıçapı 5 µm

Table 2: Test parameters for nano scratch measurements on grooved stent samples

stent groove cross section polymer coating thickness adhesion analysis nano scratch testing

Fig. 1: SEM cross-section of a grooved stent showing polymer coating located at the bottom of the groove, highlighting the challenge of coating adhesion measurement in recessed geometries.

nano scratch diamond tip 40 degree stent groove coating adhesion testing schematic

Fig. 2: Schematic of a 40° conical diamond tip designed for nano scratch testing inside stent grooves, enabling accurate adhesion measurement without sidewall interference.

Sonuçlar ve Tartışma

The stent mesh has a diameter of approximately 100 μm, comparable to a human hair. Precise positioning is therefore critical to ensure the scratch test is performed at the center of the stent mesh. The NANOVEA Mechanical Tester provides X–Y positioning accuracy down to 0.25 μm, enabling accurate test placement under the integrated optical microscope.

1. Regular Stent Samples

Nano scratch testing is performed with a progressively increasing load up to 300 mN. The full scratch track on the stent is shown in Fig. 3a, while failure behavior at different stages is presented in Fig. 3b and 3c.

Two critical loads are identified:

  • Lc1: the load at which the first visible damage appears on the coating
  • Lc2: the load at which the coating is fully removed and the substrate is exposed

The evolution of coefficient of friction (COF) and penetration depth is shown in Fig. 4, providing insight into the progression of coating failure during the test.

The first signs of coating damage appear at Lc1 ≈ 14.5 mN. As the applied load increases, the diamond tip progressively penetrates the polymer coating, resulting in a wider and deeper scratch track. During this phase, the COF increases from approximately 0.05 to 0.7.

At Lc2 ≈ 78.1 mN, the coating is fully delaminated from the metal substrate. Beyond this point, as the load continues to increase, both COF and penetration depth remain relatively stable due to the mechanical support of the underlying metal substrate.

nano scratch track stent coating progressive load adhesion testing

(a) Full Scratch Track

(b) Lc1 ≈ 14.5 mN

stent coating delamination lc2 nano scratch 78.1 mN adhesion testing

(c) Lc2 ≈ 78.1 mN

Fig. 3: Nano scratch track on a stent coating under progressively increasing load, showing (a) full scratch path, (b) initial coating failure at Lc1 ≈ 14.5 mN, and (c) complete coating delamination at Lc2 ≈ 78.1 mN.

nano scratch testing stent coating coefficient of friction depth progression adhesion failure

Fig. 4: Evolution of coefficient of friction (COF) and penetration depth during nano scratch testing of a stent coating under progressively increasing load, showing the progression of coating failure and transition to substrate support.

Failures during nano scratch testing up to a maximum load of 300 mN occur at critical loads below 100 mN. To enable a more quantitative comparison of coating performance, additional tests are performed with a maximum load of 100 mN on two stent samples, referred to as Sample 1 and Sample 2.

Fig. 5 compares the scratch tracks of Sample 1 and Sample 2 after nano scratch testing. Sample 1 exhibits the first sign of coating damage at a critical load of Lc1 ≈ 13.2 mN, while Sample 2 shows initial failure at a higher load of Lc1 ≈ 21.1 mN.

Coating delamination occurs at 62.5 mN for Sample 1. In contrast, the coating on Sample 2 remains intact throughout the test, continuing to protect the metal substrate under the same loading conditions.

This behavior is further reflected in the evolution of coefficient of friction (COF) and penetration depth, as shown in Fig. 6. When the diamond tip penetrates through the coating and contacts the metal substrate in Sample 1, the COF reaches a peak while the penetration depth decreases due to the increased stiffness of the underlying substrate.

stent coating sample 1 early failure nano scratch track delamination adhesion testing

(a) Sample 1 – Early Coating Failure

stent coating sample 2 high adhesion nano scratch track minimal damage testing

(b) Sample 2 – Improved Coating Integrity

Fig. 5: Comparison of nano scratch tracks for two stent coatings, showing (a) early coating failure and delamination in Sample 1, and (b) improved coating integrity in Sample 2 under the same loading conditions.

nano scratch testing stent coating COF depth comparison sample 1 sample 2 adhesion performance

Fig. 6: Comparison of coefficient of friction (COF) and penetration depth for Sample 1 and Sample 2 during nano scratch testing, showing earlier substrate contact and higher friction response in Sample 1, indicating weaker coating adhesion.

2. Grooved Stent Samples

As shown in Fig. 1 and Fig. 7, the grooved stent mesh has a diameter of approximately 90 μm, comparable to a human hair. The groove has a width of ~50 μm and a depth of 30 μm. This geometry presents a significant challenge for nano scratch testing, particularly for evaluating coating adhesion at the bottom of the groove.

Precise positioning is critical to locate the scratch test within the groove. The nano scratch test is performed with a progressively increasing load up to 300 mN. The full scratch tracks of grooved stent Samples 3 and 4 are compared in Fig. 7.

The critical load Lc is defined as the load at which the coating fails and the substrate becomes exposed. The evolution of normal load and penetration depth, shown in Fig. 8, provides further insight into the progression of coating failure during testing.

As the applied load increases, the diamond tip progressively penetrates the polymer coating, resulting in a deeper scratch track. When the critical load Lc is reached, the coating delaminates from the metal substrate.

Sample 3 exhibits coating failure at Lc ≈ 126 mN, while Sample 4 fails at a higher load of Lc ≈ 173 mN. This difference indicates stronger adhesion of the coating in Sample 4.

The measured critical loads enable quantitative comparison of coating adhesion performance. Under the same testing conditions, the coating on Sample 4 demonstrates higher resistance to delamination, making it the better-performing candidate in this study.

stent groove coating failure sample 3 nano scratch 126 mN adhesion testing

(c) Sample 3 – Coating Failure in Groove (Lc ≈ 126 mN)

stent groove coating adhesion sample 4 nano scratch 173 mN minimal failure testing

(d) Sample 4 – Higher Adhesion in Groove (Lc ≈ 173 mN)

Fig. 7: Nano scratch tracks inside stent grooves for Samples 3 and 4, showing (c) coating failure at Lc ≈ 126 mN in Sample 3 and (d) higher adhesion with delayed failure at Lc ≈ 173 mN in Sample 4.

(a) Sample 3 – Earlier Coating Failure (Lc ≈ 126 mN)

(b) Sample 4 – Delayed Failure and Higher Adhesion (Lc ≈ 173 mN)

Fig. 8: Evolution of normal load and penetration depth during nano scratch testing inside stent grooves for Samples 3 and 4, showing earlier coating failure in Sample 3 and delayed failure at higher load in Sample 4. The vertical green line indicates the critical load (Lc) where coating delamination occurs.

Sonuç

This study demonstrates the ability of the NANOVEA Mechanical Tester to quantitatively evaluate the cohesive and adhesive strength of polymer coatings on both regular and grooved stent geometries using nano scratch testing.

The recessed geometry of the stent grooves, approximately 50 μm wide and 30 μm deep, presents a significant challenge for coating adhesion measurement. The high X–Y positioning accuracy of 0.25 μm enables precise placement of the scratch test within these confined regions, allowing direct evaluation of coating performance where failure is most critical.

By applying a controlled, progressively increasing load, critical loads associated with coating failure can be identified and compared across samples. This approach enables reliable differentiation of coating adhesion performance and interfacial integrity, even on small, complex stent structures.

Referanslar

[I] http://www.nhlbi.nih.gov/health/health-topics/topics/stents
[II] http://www.scielo.org.mx/scielo.php?script=sci_arttext&pid=S1405-99402006000300008

Frequently Asked Questions About Stent Coating Adhesion Testing

What is stent coating adhesion testing?

Stent coating adhesion testing evaluates how strongly a polymer coating is bonded to the metal substrate of a stent. Techniques such as nano scratch testing quantify the load at which coating damage and delamination occur, providing measurable indicators of adhesion strength.

What is critical load (Lc) in nano scratch testing?

Critical load (Lc) is the applied load at which a coating fails during a scratch test.

  • Lc1 corresponds to the first visible damage in the coating
  • Lc2 indicates complete coating removal and exposure of the substrate

These values are used to quantify and compare coating adhesion performance.

Why is coating adhesion important in drug-eluting stents?

Coating adhesion directly affects the reliability of drug-eluting stents. Poor adhesion can lead to coating delamination, which may compromise controlled drug release and increase the risk of device failure.

How do you measure coating adhesion inside stent grooves?

Measuring adhesion inside stent grooves requires high positioning accuracy and appropriate indenter geometry. Nano scratch testing with sharp diamond tips allows access to recessed coating regions, enabling direct evaluation of adhesion within complex stent geometries.

What does coefficient of friction (COF) indicate in scratch testing?

The coefficient of friction (COF) reflects changes in surface interaction during the scratch test. A sudden increase in COF often indicates coating failure and contact between the indenter and the underlying metal substrate.

How can nano scratch testing compare different coating formulations?

Nano scratch testing enables direct comparison of coatings by measuring critical loads under controlled conditions. Higher critical loads indicate stronger adhesion and improved resistance to delamination, allowing selection of better-performing coating systems.

Dentist holding dental model for tooth surface roughness analysis and 3D reconstruction

Dental Surface Roughness Measurement & 3D Tooth Topography

Application Note | Dental Surface Characterization

Dental Surface Roughness Measurement and Full 3D Tooth Topography

Surface Roughness Analysis Using Non-Contact Optical Profilometry

Dental surface roughness measurement and 3D molar reconstruction using optical profilometry

Tarafından hazırlanmıştır

Walter Alabiso, PhD; Davide Morrone, MPhys; Andrew Shore, MA

Giriş

The ability to accurately characterize tooth surfaces, including micro-roughness and 3D surface topography at the nanometer scale, enables advanced research and applications in orthodontics and dental materials science. Non-contact optical profilometry provides a precise method for measuring dental surface roughness and analyzing tooth surface morphology without damaging delicate structures. These measurements support the development of composite dental materials that replicate the natural surface roughness of enamel, as well as the design and fabrication of patient-specific dental casts and restorative components.

Low surface roughness plays a primary role in limiting bacterial adhesion and plaque formation, thereby reducing the risk of cavities. An increase in average roughness (Ra) above 2 µm leads to a steep increase in biofilm formation in vivo.¹ An Ra of 0.2 µm is considered the threshold value below which no further reduction in bacterial adhesion can be expected.²

Reconstruction of the tooth’s 3D surface topography enables the fabrication of dental casts, which are essential for accurate diagnosis, treatment planning, and the fabrication of dental appliances.

Non-Contact Optical Profilometry for Dental Surface Analysis

The present study illustrates the potential of NANOVEA’s high-precision non-contact optical profilometers for dental surface roughness measurement and 3D tooth topography analysis. Chromatic Light technology offers significant advantages over classical touch probe techniques. It acquires data points from deep crevices and complex geometries without introducing measurement errors or artifacts caused by local plastic deformation and without requiring extensive data manipulation.

Compared to focus variation systems, single-point optical sensing provides superior lateral and height accuracy, with X/Y resolution below 0.5 µm, maximum vertical resolution of 1.9 nm, and the ability to measure surface angles up to 87°. The technique is effective on transparent, opaque, specular, diffusive, polished, and rough dental surfaces, making it well suited for comprehensive dental surface characterization.

Measurement Method

Bu uygulamada NANOVEA JR25 Non-Contact Optical Profiler was used to analyze the surface roughness and 3D surface topography of an adult human molar previously affected by tooth decay. The side of the tooth was scanned using a PS2–MG140 single-point optical sensor to measure surface roughness parameters over a defined region of interest and along multiple line profiles.

The crown of the tooth was then scanned and reconstructed using a PS5–MG35 single-point optical sensor, which is suited for larger-area acquisition and full 3D tooth topography measurement.


NANOVEA JR25 Portable
Optik Profilometre

Surface Measurement Using NANOVEA Optical Profilometer

Surface roughness measurements were performed on the lateral side of the molar crown, followed by full 3D reconstruction of the crown surface. Separate single-point optical sensors were used to optimize measurement accuracy for both localized roughness analysis and large-area surface topography acquisition.

PS2 – MG140

Surface roughness analysis by area and parallel line profiles on the side of the tooth’s crown.

PS5 – MG35

Full 3D surface reconstruction of the tooth’s crown.

Ölçüm Parametreleri

The following measurement parameters were used for localized surface roughness analysis and full 3D surface reconstruction of the molar crown using NANOVEA single-point optical sensors.

ParameterRoughness Analysis (Area)Roughness Analysis (Profiles)Full 3D Reconstruction
Optical PenPS2-MG140PS2-MG140PS5-MG35
Z-Range [µm]30030010000
X-Distance [mm]2.003.007.50
X-Step Size [µm]1.701.7010.00
Y-Distance [mm]2.001.007.00
Y-Step Size [µm]1.70100.0010.00
Averaging (Avg)111
Measurement TypeDirectDirectDirect
Acquisition ModeSingle FrequencySingle FrequencyDual Frequency
Acquisition Rate [Hz]200200100–400
Light Intensity [%]100100100

Optical Profilometry Results

Surface Roughness Analysis (AREA)

 The single-point optical sensor PS2 was used to investigate fine features of the tooth’s side surface. The following picture represents a false-color 2D map of the scanned region:

False-color 2D height map of scanned tooth surface region

A least-squares degree-8 polynomial form removal was applied to isolate the surface roughness component. The roughness filters S-Gaussian 2.5 µm and L-Gaussian 0.8 mm were then applied according to ISO 25178. The resulting filtered surface and corresponding roughness parameters are presented below.

ISO 25178 – Roughness (S-L)
S-filter (λs): Gaussian, 2.5 µm
F: [Workflow] Form removed (LS-poly 8)
L-filter (λc): Gaussian, 0.8 mm
Height Parameters
Sq2.433µmKök ortalama kare yüksekliği
Ssk-0.102 Çarpıklık
Sku3.715 Kurtosis
Sp18.861µmMaksimum tepe yüksekliği
Sv16.553µmMaximum pit depth
Sz35.414µmMaksimum yükseklik
Sa1.888µmAritmetik ortalama yükseklik

The average surface roughness Sa is 1.888 µm, while the peak-to-valley height Sz reaches 35.414 µm.

A 3D surface rendering of the filtered area is shown below for visualization.

3D rendering of ISO 25178 filtered tooth surface roughness

Roughness Analysis (Profiles)

Surface roughness profiles were measured using a series of 11 parallel line scans along the X direction on the side of the tooth. The false-color 2D surface map of the raw scan is shown below.

False-color 2D raw scan of tooth surface for line roughness profiles

The surface form was removed using a least-squares 8-degree polynomial prior to applying the metrological filters, leaving the residual surface shown below.

A statistical analysis of the measured surface roughness profiles reveals the following line roughness parameters.

Overlay of multiple tooth surface roughness profiles for statistical analysis

ISO 4287 – Roughness (S-L)
F: Hiçbiri
S-filter (λs): Gaussian, 2.5 µm
L-filter (λc): Gaussian, 0.8 mm
Evaluation length: All λc (3)
Amplitude Parameters – Roughness Profile
  DescriptionMeanStd devMinMax
RpµmMaximum peak height of the roughness profile5.6830.7614.3156.610
RvµmMaximum valley depth of the roughness profile6.2421.0094.7018.438
RzµmMaximum height of roughness profile11.9251.6769.12315.048
RaµmArithmetic mean deviation of the roughness profile2.0630.2971.7102.629
RqµmRoot-mean-square (RMS) deviation of the roughness profile2.5230.3612.0573.175

ISO 4287 – Roughness (S-L)
F: Hiçbiri
S-filter (λs): Gaussian, 2.5 µm
L-filter (λc): Gaussian, 0.8 mm
Evaluation length: All λc (3)
Amplitude Parameters – Roughness Profile
Rpµm
Maximum peak height of the roughness profile
Mean5.683
Std dev0.761
Min4.315
Max6.610
Rvµm
Maximum valley depth of the roughness profile
Mean6.242
Std dev1.009
Min4.701
Max8.438
Rzµm
Maximum height of roughness profile
Mean11.925
Std dev1.676
Min9.123
Max15.048
Raµm
Arithmetic mean deviation of the roughness profile
Mean2.063
Std dev0.297
Min1.710
Max2.629
Rqµm
Root-mean-square (RMS) deviation of the roughness profile
Mean2.523
Std dev0.361
Min2.057
Max3.175

The value of Ra is consistent with the Sa value extracted from the surface area measurement.

Different metrological filters can be applied to distinguish between macroscopic waviness and microscopic surface roughness. For example, a coarser filter cut-off, such as the 8 mm cut-off used with the Robust Gaussian order-2 filter, produces a smoother waviness profile (red) that is less sensitive to sharp local variations and follows the original surface profile more loosely.

Comparison of waviness and roughness profiles on tooth surface using coarse filter

Alternatively, a finer cut-off (e.g., 0.08 mm) enables the analysis of micro-roughness by removing the waviness component that follows the original profile at a larger scale, leaving the finer surface roughness features of the tooth visible.

The microroughness analysis obtained using a 0.08 mm L-Gaussian filter is presented below.

Final microroughness profile of tooth surface after filtering

ISO 4287 – Roughness (S-L)
F: Hiçbiri
S-filter (λs): Gaussian, 2.5 µm
L-filter (λc): Gaussian, 0.08 mm
Evaluation length: All λc (37)
Amplitude Parameters – Roughness Profile
  DescriptionMeanStd devMinMax
RpµmMaximum peak height of the roughness profile1.5820.1221.3421.748
RvµmMaximum valley depth of the roughness profile1.4660.1191.2541.661
RzµmMaximum height of roughness profile3.0490.1962.8203.409
RaµmArithmetic mean deviation of the roughness profile0.4950.0470.4230.597
RqµmRoot-mean-square (RMS) deviation of the roughness profile0.6430.0560.5620.762

ISO 4287 – Roughness (S-L)
F: Hiçbiri
S-filter (λs): Gaussian, 2.5 µm
L-filter (λc): Gaussian, 0.8 mm
Evaluation length: All λc (3)
Amplitude Parameters – Roughness Profile
Rpµm
Maximum peak height of the roughness profile
Mean5.683
Std dev0.761
Min4.315
Max6.610
Rvµm
Maximum valley depth of the roughness profile
Mean6.242
Std dev1.009
Min4.701
Max8.438
Rzµm
Maximum height of roughness profile
Mean11.925
Std dev1.676
Min9.123
Max15.048
Raµm
Arithmetic mean deviation of the roughness profile
Mean2.063
Std dev0.297
Min1.710
Max2.629
Rqµm
Root-mean-square (RMS) deviation of the roughness profile
Mean2.523
Std dev0.361
Min2.057
Max3.175

Full 3D Tooth Surface Topography Reconstruction

The extended Z-scan range of the PS5 optical sensor enables high-fidelity scanning of the entire tooth crown surface. The resulting 3D surface topography is shown below.

False-color surface topography map of full tooth crown measured with optical profilometer

2D VIEW: 2D surface map of the tooth crown measured with optical profilometry

3D surface reconstruction of molar crown from optical profilometer scan

3D VIEW: High-fidelity 3D rendering of the molar crown surface obtained with optical profilometry

Sonuç

In this application, the NANOVEA JR25 Non-Contact Optical Profiler was used to measure the surface roughness and 3D surface topography of an adult human molar.

Both the area scan and the line profile analysis revealed a roughness Rq of approximately 2.5 µm and an Ra of about 1.9–2.0 µm. These values are consistent with results reported in the literature.³ The use of a narrower L-Gaussian filter with an 80 µm cut-off enabled further investigation of micro-roughness, revealing an Rq of 0.643 µm and an Ra of 0.495 µm.

The full 3D surface topography of the molar crown was reconstructed with high fidelity. The high measurement resolution allows detection of fine surface features and crevices. The resulting surface data can be easily processed and exported as STL files, enabling the design and fabrication of customized dental devices and restorative components.

Referanslar

[1] Shin, B.W., et al. Surface Roughness of Prefabricated Pediatric Zirconia Crowns Following Simulated Toothbrushing. Pediatric Dentistry 44.5 (2022): 363–367.
[2] Bollen, C.M.L., Paul Lambrechts, and Marc Quirynen. Comparison of surface roughness of oral hard materials to the threshold surface roughness for bacterial plaque retention: A review of the literature. Dental Materials 13.4 (1997): 258–269.
[3] Suputtamongkol, K., et al. Surface roughness resulting from wear of lithia-disilicate-based posterior crowns. Wear 269.3–4 (2010): 317–322.

Frequently Asked Questions About Dental Surface Roughness Measurement

What is dental surface roughness measurement?

Dental surface roughness measurement quantifies the microscopic texture of tooth surfaces using parameters such as Ra, Rq, and Sa. Optical profilometers measure these features without contacting the surface, allowing accurate analysis of enamel, restorative materials, and dental crowns.

Why use optical profilometry to measure tooth roughness?

Optical profilometry provides non-contact surface measurement with nanometer-scale vertical resolution. It captures 2D surface maps and full 3D surface topography of dental structures without damaging soft or polished surfaces.

What roughness parameters are used for dental surface analysis?

Common roughness parameters include Ra (arithmetic mean roughness), Rq (root mean square roughness), Sa (areal roughness), and Sz (maximum surface height). These parameters help evaluate enamel wear, plaque adhesion risk, and the performance of restorative materials.

Why is surface roughness important in dentistry?

Surface roughness affects plaque retention, wear resistance, and the long-term performance of dental restorations. Controlling micro-roughness can reduce bacterial adhesion and improve the durability of dental materials.

Need Reliable Surface Roughness Measurement for Dental Materials?

Bilye Dövülmüş Yüzey Analizi

PİLLENMİŞ YÜZEY ANALİZİ

3D TEMASSIZ PROFİLOMETRE KULLANIMI

Tarafından hazırlanmıştır

CRAIG LEISING

GİRİŞ

Bilyalı dövme, bir alt tabakanın küresel metal, cam veya seramik boncuklarla (genelde "shot" olarak anılır) yüzeyde plastisite oluşturmayı amaçlayan bir kuvvetle bombardımana tutulduğu bir işlemdir. Dövme öncesi ve sonrası özelliklerin analiz edilmesi, süreç kavrayışını ve kontrolünü geliştirmek için çok önemli bilgiler sağlar. Yüzey pürüzlülüğü ve çekimin bıraktığı çukurların kapsama alanı özellikle ilgi çekici yönlerdir.

Shot-Peened Yüzey Analizi için 3D Temassız Profilometrenin Önemi

Geleneksel olarak bilyalı dövmeli yüzey analizi için kullanılan geleneksel temaslı profilometrelerin aksine, 3D temassız ölçüm, kapsama alanı ve yüzey topografyasının daha kapsamlı anlaşılmasını sağlamak için eksiksiz bir 3D görüntü sağlar. 3D yetenekleri olmadan, bir inceleme yalnızca 2D bilgilerine dayanacaktır ve bu da bir yüzeyin karakterize edilmesi için yeterli değildir. Topografyayı, kapsama alanını ve pürüzlülüğü 3 boyutlu olarak anlamak, dövme sürecini kontrol etmek veya iyileştirmek için en iyi yaklaşımdır. NANOVEA'lar 3D Temassız Profilometreler İşlenmiş ve dövülmüş yüzeylerde bulunan dik açıları ölçmek için benzersiz bir yeteneğe sahip Chromatic Light teknolojisini kullanır. Ayrıca diğer teknikler prob teması, yüzey değişimi, açı veya yansıma nedeniyle güvenilir veri sağlayamadığında NANOVEA Profilometreler başarılı olur.

ÖLÇÜM HEDEFI

Bu uygulamada, NANOVEA ST400 Temassız Profilometre, karşılaştırmalı bir inceleme için ham maddeyi ve iki farklı şekilde dövülmüş yüzeyi ölçmek için kullanılır. 3D yüzey taramasından sonra otomatik olarak hesaplanabilen sonsuz bir yüzey parametreleri listesi vardır. Burada, 3B yüzeyi gözden geçireceğiz ve pürüzlülük, çukurlar ve yüzey alanını ölçmek ve araştırmak da dahil olmak üzere daha fazla analiz için ilgi alanlarını seçeceğiz.

NANOVEA ST400 Standart
Optik 3D Profilometre

ÖRNEK

Bilyeli Çekiçleme Yüzey Testi

SONUÇLAR

ÇELİK YÜZEY

Bilyeli Çarpma ile Pürüzlendirilmiş Yüzey Pürüzlülüğü
Bilyeli Çekiçleme ile İşlenmiş Yüzey Karakterizasyonu

ISO 25178 3D PÜRÜZLÜLÜK PARAMETRELERİ

SA 0,399 mikron Ortalama Pürüzlülük
Sq 0,516 mikron RMS Pürüzlülüğü
Sz 5.686 mikron Maksimum Zirveden Vadiye
Sp 2,976 mikron Maksimum Tepe Yüksekliği
Sv 2,711 mikron Maksimum Çukur Derinliği
Sku 3.9344 Kurtosis
Ssk -0.0113 Çarpıklık
Sal 0,0028 mm Otomatik Korelasyon Uzunluğu
Sokak 0.0613 Doku En Boy Oranı
Sdar 26.539 mm² Yüzey alanı
Svk 0,589 mikron Azaltılmış Vadi Derinliği
 

SONUÇLAR

Dövülmüş YÜZEY 1

Bilyeli Çekiçleme Yüzey Profili
Bilyeli Çekiçleme Yüzey Profilometrisi

YÜZEY KAPLAMASI 98.105%

Bilyeli Çekiçleme Yüzey Çalışması

ISO 25178 3D PÜRÜZLÜLÜK PARAMETRELERİ

Sa 4.102 mikron Ortalama Pürüzlülük
Sq 5.153 mikron RMS Pürüzlülüğü
Sz 44.975 mikron Maksimum Zirveden Vadiye
Sp 24.332 mikron Maksimum Tepe Yüksekliği
Sv 20.644 mikron Maksimum Çukur Derinliği
Sku 3.0187 Kurtosis
Ssk 0.0625 Çarpıklık
Sal 0,0976 mm Otomatik Korelasyon Uzunluğu
Sokak 0.9278 Doku En Boy Oranı
Sdar 29.451 mm² Yüzey alanı
Svk 5.008 mikron Azaltılmış Vadi Derinliği

SONUÇLAR

Dövülmüş YÜZEY 2

Bilyeli Çekiçleme Yüzey Testi
Şot Peenli Yüzey Analizi

YÜZEY KAPLAMASI 97.366%

Bilyeli Çekiçleme Yüzey Metrolojisi

ISO 25178 3D PÜRÜZLÜLÜK PARAMETRELERİ

Sa 4.330 mikron Ortalama Pürüzlülük
Sq 5.455 mikron RMS Pürüzlülüğü
Sz 54.013 mikron Maksimum Zirveden Vadiye
Sp 25.908 mikron Maksimum Tepe Yüksekliği
Sv 28.105 mikron Maksimum Çukur Derinliği
Sku 3.0642 Kurtosis
Ssk 0.1108 Çarpıklık
Sal 0,1034 mm Otomatik Korelasyon Uzunluğu
Sokak 0.9733 Doku En Boy Oranı
Sdar 29.623 mm² Yüzey alanı
Svk 5.167 mikron Azaltılmış Vadi Derinliği

SONUÇ

Bu bilyeli yüzey analizi uygulamasında, NANOVEA ST400 3D Temassız Profil Oluşturucunun, dövülmüş bir yüzeyin hem topografyasını hem de nanometre ayrıntılarını tam olarak nasıl karakterize ettiğini gösterdik. Hem Yüzey 1'in hem de Yüzey 2'nin, ham maddeye kıyasla burada bildirilen tüm parametreler üzerinde önemli bir etkiye sahip olduğu açıktır. Görüntülerin basit bir görsel incelemesi, yüzeyler arasındaki farklılıkları ortaya çıkarır. Bu, kapsama alanı ve listelenen parametreler gözlemlenerek daha da doğrulanır. Yüzey 2 ile karşılaştırıldığında, Yüzey 1 daha düşük bir ortalama pürüzlülük (Sa), daha sığ çentikler (Sv) ve azaltılmış yüzey alanı (Sdar) sergiler, ancak biraz daha yüksek kapsama alanı gösterir.

Bu 3B yüzey ölçümlerinden, ilgili alanlar kolayca belirlenebilir ve Pürüzlülük, Bitiş, Doku, Şekil, Topografya, Yassılık, Çarpıklık, Düzlemsellik, Hacim, Adım Yüksekliği ve diğerleri dahil olmak üzere kapsamlı bir ölçüm dizisine tabi tutulabilir. Ayrıntılı analiz için bir 2B kesit hızla seçilebilir. Bu bilgi, eksiksiz bir yüzey ölçüm kaynakları yelpazesi kullanılarak, dövülmüş yüzeylerin kapsamlı bir şekilde araştırılmasına olanak tanır. Belirli ilgi alanları, entegre bir AFM modülü ile daha fazla incelenebilir. NANOVEA 3D Profilometreler, 200 mm/sn'ye varan hızlar sunar. Boyut, hız, tarama özellikleri açısından özelleştirilebilirler ve hatta Sınıf 1 Temiz Oda standartlarına bile uyum sağlayabilirler. İndeksleme Konveyörü ve Inline veya Online kullanım için entegrasyon gibi seçenekler de mevcuttur.

Bu notta gösterilen numuneyi sağlayan IMF'den Bay Hayden'a özel teşekkürler. Industrial Metal Finishing Inc. | indmetfin.com

Boya Yüzey Morfolojisi

BOYA YÜZEY MORFOLOJİSİ

OTOMATİK GERÇEK ZAMANLI GELİŞİM İZLEME
NANOVEA 3D PROFİLOMETRE KULLANIMI

Boya Yüzey Morfolojisi

Tarafından hazırlanmıştır

DUANJIE LI, PhD

GİRİŞ

Boyanın koruyucu ve dekoratif özellikleri, otomotiv, denizcilik, askeriye ve inşaat dahil olmak üzere çeşitli endüstrilerde önemli bir rol oynamaktadır. Korozyon direnci, UV koruması ve aşınma direnci gibi istenen özellikleri elde etmek için boya formülleri ve mimarileri dikkatli bir şekilde analiz edilir, değiştirilir ve optimize edilir.

KURUTMA BOYA YÜZEY MORFOLOJİSİ ANALİZİ İÇİN 3D TEMASSIZ PROFİLOMETRE ÖNEMİ

Boya genellikle sıvı halde uygulanır ve solventlerin buharlaştırılmasını ve sıvı boyanın katı bir filme dönüştürülmesini içeren bir kurutma işlemine tabi tutulur. Kurutma işlemi sırasında, boya yüzeyi kademeli olarak şeklini ve dokusunu değiştirir. Boyanın yüzey gerilimini ve akış özelliklerini değiştirmek için katkı maddeleri kullanılarak farklı yüzey kaplamaları ve dokular geliştirilebilir. Ancak, kötü formüle edilmiş bir boya tarifi veya uygun olmayan yüzey işlemi durumlarında, istenmeyen boya yüzey arızaları meydana gelebilir.

Kuruma süresi boyunca boya yüzey morfolojisinin yerinde doğru bir şekilde izlenmesi, kuruma mekanizmasına doğrudan bir bakış sağlayabilir. Dahası, yüzey morfolojilerinin gerçek zamanlı gelişimi, 3D baskı gibi çeşitli uygulamalarda çok faydalı bir bilgidir. NANOVEA 3D Temassız Profilometreler Malzemelerin boya yüzey morfolojisini numuneye dokunmadan ölçerek kayan kalem gibi temas teknolojilerinin neden olabileceği şekil değişikliklerini önleyin.

ÖLÇÜM HEDEFI

Bu uygulamada, yüksek hızlı hat optik sensörü ile donatılmış NANOVEA ST500 Temassız Profilometre, 1 saatlik kuruma süresi boyunca boya yüzey morfolojisini izlemek için kullanılır. NANOVEA Temassız Profilometrenin, sürekli şekil değiştiren malzemelerin otomatikleştirilmiş gerçek zamanlı 3D profil ölçümünü sağlama yeteneğini sergiliyoruz.

NANOVEA ST500 Geniş Alan
Optik 3D Profilometre

SONUÇLAR & TARTIŞMA

Boya, bir metal levhanın yüzeyine uygulandı ve hemen ardından, yüksek hızlı bir hat sensörü ile donatılmış NANOVEA ST500 Temassız Profilometre kullanılarak yerinde kuruyan boyanın morfoloji gelişiminin otomatik ölçümleri yapıldı. 3D yüzey morfolojisini belirli zaman aralıklarında otomatik olarak ölçmek ve kaydetmek için bir makro programlanmıştır: 0, 5, 10, 20, 30, 40, 50 ve 60 dakika. Bu otomatikleştirilmiş tarama prosedürü, kullanıcıların belirlenen prosedürleri sırayla çalıştırarak tarama görevlerini otomatik olarak gerçekleştirmesini sağlayarak manuel test veya tekrarlanan taramalara kıyasla eforu, zamanı ve olası kullanıcı hatalarını önemli ölçüde azaltır. Bu otomasyon, farklı zaman aralıklarında çoklu taramaları içeren uzun vadeli ölçümler için son derece yararlı olduğunu kanıtlıyor.

Optik hat sensörü, ŞEKİL 1'de gösterildiği gibi 192 noktadan oluşan parlak bir çizgi oluşturur. Bu 192 ışık noktası numune yüzeyini aynı anda tarayarak tarama hızını önemli ölçüde artırır. Bu, her bir ayrı tarama sırasında önemli yüzey değişikliklerinden kaçınmak için her 3B taramanın hızlı bir şekilde tamamlanmasını sağlar.

3D Profilometre kullanarak Boya Kaplama Analizi

ŞEKİL 1: Kuruyan boyanın yüzeyini tarayan optik hat sensörü.

Temsili zamanlarda kuruyan boya topografyasının yanlış renk görünümü, 3B görünümü ve 2B profili sırasıyla ŞEKİL 2, ŞEKİL 3 ve ŞEKİL 4'te gösterilmektedir. Görüntülerdeki yanlış renk, kolayca fark edilemeyen özelliklerin algılanmasını kolaylaştırır. Farklı renkler, numune yüzeyinin farklı alanlarındaki yükseklik değişikliklerini temsil eder. 3D görünüm, kullanıcıların boya yüzeyini farklı açılardan gözlemlemesi için ideal bir araç sağlar. Testin ilk 30 dakikasında, boya yüzeyindeki sahte renkler kademeli olarak daha sıcak tonlardan daha soğuk tonlara doğru değişir ve bu süre içinde boyda kademeli bir azalma olduğunu gösterir. Boyayı 30 ve 60 dakikada karşılaştırırken hafif renk değişiminin gösterdiği gibi bu süreç yavaşlar.

Boya kuruma süresinin bir fonksiyonu olarak ortalama numune yüksekliği ve pürüzlülük Sa değerleri ŞEKİL 5'te çizilmiştir. 0, 30 ve 60 dakika kuruma süresinden sonra boyanın tam pürüzlülük analizi TABLO 1'de listelenmiştir. boya yüzeyinin ortalama yüksekliği, kuruma süresinin ilk 30 dakikasında hızla 471 µm'den 329 µm'ye düşer. Yüzey dokusu, çözücünün buharlaşmasıyla aynı anda gelişir ve pürüzlülük Sa değerinin 7,19'dan 22,6 µm'ye yükselmesine yol açar. Boya kurutma işlemi daha sonra yavaşlar ve 60 dakikada numune yüksekliğinin ve Sa değerinin kademeli olarak sırasıyla 317 µm ve 19,6 µm'ye düşmesine neden olur.

Bu çalışma, NANOVEA 3D Temassız Profilometrenin, kuruyan boyanın 3D yüzey değişikliklerini gerçek zamanlı olarak izleme konusundaki yeteneklerini vurgulayarak, boya kurutma işlemine ilişkin değerli bilgiler sağlar. Profilometre, numuneye dokunmadan yüzey morfolojisini ölçerek, kayan prob ucu gibi temas teknolojileriyle meydana gelebilecek, kurumamış boyaya şekil değişikliklerinin getirilmesini önler. Bu temassız yaklaşım, kuruyan boya yüzeyi morfolojisinin doğru ve güvenilir analizini sağlar.

Boya Yüzey Morfolojisi
Boya Kaplama Morfolojisi

ŞEKİL 2: Farklı zamanlarda kuruyan boya yüzey morfolojisinin gelişimi.

Boya Yüzeyinin Karakterizasyonu
Boya Yüzey Profili
Boya Yüzey Analizi

ŞEKİL 3: Farklı kuruma sürelerinde boya yüzeyi gelişiminin 3 boyutlu görünümü.

Boya Yüzeyi Profilometrisi

ŞEKİL 4: Farklı kuruma sürelerinden sonra boya numunesi boyunca 2B profil.

Boya Yüzeyi Çalışması

ŞEKİL 5: Boya kuruma süresinin bir fonksiyonu olarak ortalama numune yüksekliği ve pürüzlülük değeri Sa'nın gelişimi.

ISO 25178 - Yüzey Dokusu Parametreleri

Kuruma süresi (dk) 0 5 10 20 30 40 50 60
Kare (µm) 7.91 9.4 10.8 20.9 22.6 20.6 19.9 19.6
Sku 26.3 19.8 14.6 11.9 10.5 9.87 9.83 9.82
Hız (µm) 97.4 105 108 116 125 118 114 112
Sv (µm) 127 70.2 116 164 168 138 130 128
Sz (µm) 224 175 224 280 294 256 244 241
Sa (µm) 4.4 5.44 6.42 12.2 13.3 12.2 11.9 11.8

kare – Kök ortalama kare yüksekliği | Sku – Kurtosis | sp- Maksimum tepe yüksekliği | Sev – Maksimum çukur yüksekliği | Sz- Maksimum yükseklik | Sev – Aritmetik ortalama yükseklik

TABLO 1: Farklı kuruma sürelerinde boya pürüzlülüğü.

SONUÇ

Bu uygulamada, kurutma işlemi sırasında boya yüzeyi morfolojisinin gelişimini izlemede NANOVEA ST500 3D Temassız Profilometrenin yeteneklerini sergiledik. Numune yüzeyini aynı anda tarayan 192 ışık noktalı bir çizgi oluşturan yüksek hızlı optik çizgi sensörü, eşsiz doğruluk sağlarken çalışmayı zamandan tasarruf ettirdi.

Edinme yazılımının makro işlevi, yerinde 3B yüzey morfolojisinin otomatik ölçümlerinin programlanmasına izin vererek, belirli hedef zaman aralıklarında çoklu taramaları içeren uzun vadeli ölçümler için özellikle yararlı hale getirir. Kullanıcı hataları için zamanı, çabayı ve potansiyeli önemli ölçüde azaltır. Yüzey morfolojisindeki aşamalı değişiklikler, boya kurudukça sürekli olarak izlenir ve gerçek zamanlı olarak kaydedilir, bu da boya kuruma mekanizması hakkında değerli bilgiler sağlar.

Burada gösterilen veriler, analiz yazılımında bulunan hesaplamaların yalnızca bir kısmını temsil etmektedir. NANOVEA Profilometreler, şeffaf, koyu, yansıtıcı veya opak olsun, hemen hemen her yüzeyi ölçebilir.

3D Profilometri Kullanarak Pürüzlülük Haritalama Denetimi

PÜRÜZLÜLÜK HARITALAMA DENETIMI

3 BOYUTLU PROFILOMETRI KULLANARAK

Tarafından hazırlanmıştır

DUANJIE, PhD

GİRİŞ

Yüzey pürüzlülüğü ve dokusu, bir ürünün nihai kalitesini ve performansını etkileyen kritik faktörlerdir. Yüzey pürüzlülüğü, dokusu ve tutarlılığının tam olarak anlaşılması, en iyi işleme ve kontrol önlemlerinin seçilmesi için gereklidir. Kusurlu ürünleri zamanında tespit etmek ve üretim hattı koşullarını optimize etmek için ürün yüzeylerinin hızlı, ölçülebilir ve güvenilir hat içi denetimine ihtiyaç vardır.

HAT İÇİ YÜZEY DENETİMİ İÇİN 3 BOYUTLU TEMASSIZ PROFİLOMETRENİN ÖNEMİ

Ürünlerdeki yüzey kusurları malzeme işleme ve ürün imalatından kaynaklanır. Hat içi yüzey kalite denetimi, son ürünlerin en sıkı kalite kontrolünü sağlar. NANOVEA 3D Temassız Optik Profil Oluşturucular Bir numunenin pürüzlülüğünü temassız olarak belirlemek için benzersiz kapasiteye sahip Kromatik Işık teknolojisini kullanır. Çizgi sensörü, geniş bir yüzeyin 3 boyutlu profilinin yüksek hızda taranmasını sağlar. Analiz yazılımı tarafından gerçek zamanlı olarak hesaplanan pürüzlülük eşiği, hızlı ve güvenilir bir başarılı/başarısız aracı olarak hizmet eder.

ÖLÇÜM HEDEFI

Bu çalışmada, yüksek hızlı bir sensörle donatılmış NANOVEA ST400, NANOVEA'nın kapasitesini göstermek için kusurlu bir Teflon numunesinin yüzeyini incelemek için kullanılmıştır.

Temassız Profilometreler, bir üretim hattında hızlı ve güvenilir yüzey denetimi sağlar.

NANOVEA

ST400

SONUÇLAR & TARTIŞMA

3 Boyutlu Yüzey Analizi Pürüzlülük Standart Numune

Bir Pürüzlülük Standardının yüzeyi, ŞEKİL 1'de gösterildiği gibi 192 noktadan oluşan parlak bir çizgi oluşturan yüksek hızlı bir sensörle donatılmış bir NANOVEA ST400 kullanılarak taranmıştır. Bu 192 nokta numune yüzeyini aynı anda tarayarak tarama hızının önemli ölçüde artmasını sağlar.

ŞEKİL 2'de Pürüzlülük Standardı Numunesinin Yüzey Yüksekliği Haritası ve Pürüzlülük Dağılımı Haritasının sahte renkli görünümleri gösterilmektedir. ŞEKİL 2a'da Pürüzlülük Standardı, standart pürüzlülük bloklarının her birinde değişen renk gradyanıyla temsil edildiği üzere hafif eğimli bir yüzey sergilemektedir. ŞEKİL 2b'de, rengi bloklardaki pürüzlülüğü temsil eden farklı pürüzlülük bloklarında homojen pürüzlülük dağılımı gösterilmektedir.

ŞEKİL 3, Analiz Yazılımı tarafından farklı Pürüzlülük Eşiklerine dayalı olarak oluşturulan Başarılı/Başarısız Haritalarının örneklerini göstermektedir. Pürüzlülük blokları, yüzey pürüzlülükleri belirli bir eşik değerinin üzerinde olduğunda kırmızı renkle vurgulanır. Bu, kullanıcının bir numune yüzey kalitesinin kalitesini belirlemek için bir pürüzlülük eşiği ayarlaması için bir araç sağlar.

ŞEKİL 1: Pürüzlülük Standardı örneği üzerinde optik çizgi sensörü taraması

a. Yüzey Yükseklik Haritası:

b. Pürüzlülük Haritası:

ŞEKİL 2: Pürüzlülük Standart Numunesinin Yüzey Yüksekliği Haritası ve Pürüzlülük Dağılımı Haritasının yanlış renk görünümleri.

ŞEKİL 3: Pürüzlülük Eşiğine dayalı Başarılı/Başarısız Haritası.

Kusurlu Bir Teflon Numunesinin Yüzey Kontrolü

Teflon numune yüzeyinin Yüzey Yükseklik Haritası, Pürüzlülük Dağılım Haritası ve Geçer/Kalır Pürüzlülük Eşik Haritası ŞEKİL 4'te gösterilmektedir. Teflon Numunesi, Yüzey Yüksekliği Haritasında gösterildiği gibi numunenin sağ merkezinde bir sırt formuna sahiptir.

a. Yüzey Yükseklik Haritası:

ŞEKİL 4b'nin paletindeki farklı renkler yerel yüzeydeki pürüzlülük değerini temsil etmektedir. Pürüzlülük Haritası, Teflon numunesinin sağlam alanında homojen bir pürüzlülük sergilemektedir. Bununla birlikte, girintili halka ve aşınma izi şeklindeki kusurlar parlak renklerle vurgulanmıştır. Kullanıcı, ŞEKİL 4c'de gösterildiği gibi yüzey kusurlarını bulmak için kolayca bir Geçer/Kalır pürüzlülük eşiği ayarlayabilir. Böyle bir araç, kullanıcıların üretim hattındaki ürün yüzey kalitesini yerinde izlemelerine ve kusurlu ürünleri zamanında keşfetmelerine olanak tanır. Gerçek zamanlı pürüzlülük değeri, ürünler hat içi optik sensörden geçerken hesaplanır ve kaydedilir, bu da kalite kontrol için hızlı ama güvenilir bir araç olarak hizmet edebilir.

b. Pürüzlülük Haritası:

c. Geçer/Kalır Pürüzlülük Eşik Haritası:

ŞEKİL 4: Yüzey Yükseklik Haritası, Pürüzlülük Dağılım Haritası ve Teflon numune yüzeyinin Başarılı/Başarısız Pürüzlülük Eşik Haritası.

SONUÇ

Bu uygulamada, optik çizgi sensörü ile donatılmış NANOVEA ST400 3D Temassız Optik Profilleyicinin etkili ve verimli bir şekilde güvenilir bir kalite kontrol aracı olarak nasıl çalıştığını gösterdik.

Optik çizgi sensörü, numune yüzeyini aynı anda tarayan 192 noktadan oluşan parlak bir çizgi oluşturarak tarama hızını önemli ölçüde artırır. Ürünlerin yüzey pürüzlülüğünü yerinde izlemek için üretim hattına monte edilebilir. Pürüzlülük eşiği, ürünlerin yüzey kalitesini belirlemek için güvenilir bir kriter olarak çalışır ve kullanıcıların kusurlu ürünleri zamanında fark etmelerini sağlar.

Burada gösterilen veriler, analiz yazılımında bulunan hesaplamaların yalnızca bir kısmını temsil etmektedir. NANOVEA Profilometreler, Yarı İletken, Mikroelektronik, Güneş, Fiber Optik, Otomotiv, Havacılık ve Uzay, Metalurji, İşleme, Kaplama, İlaç, Biyomedikal, Çevre ve diğer birçok alanda hemen hemen her yüzeyi ölçer.

Taşınabilir 3D Profilometre Kullanarak Kaynak Yüzeyi Denetimi

WELd yüzey denetimi

portati̇f 3 boyutlu profi̇lometre kullanimi

Tarafından hazırlanmıştır

CRAIG LEISING

GİRİŞ

Tipik olarak görsel inceleme ile yapılan belirli bir kaynağın aşırı hassasiyetle incelenmesi kritik hale gelebilir. Hassas analiz için spesifik ilgi alanları arasında, sonraki muayene prosedürlerinden bağımsız olarak yüzey çatlakları, gözeneklilik ve doldurulmamış kraterler bulunur. Boyut/şekil, hacim, pürüzlülük, boyut vb. gibi kaynak özelliklerinin tümü kritik değerlendirme için ölçülebilir.

KAYNAK YÜZEYİ DENETİMİNDE 3 BOYUTLU TEMASSIZ PROFİLOMETRENİN ÖNEMİ

NANOVEA, dokunma probları veya interferometri gibi diğer tekniklerin aksine 3D Temassız ProfilometreEksenel kromatizmi kullanarak neredeyse her yüzeyi ölçebilir, açık aşamalandırma nedeniyle numune boyutları büyük ölçüde değişebilir ve numune hazırlamaya gerek yoktur. Nanodan makroya kadar aralık, yüzey profili ölçümü sırasında numune yansımasından veya emiliminden sıfır etkiyle elde edilir, yüksek yüzey açılarını ölçme konusunda gelişmiş bir yeteneğe sahiptir ve sonuçların yazılımla manipülasyonu yoktur. Herhangi bir malzemeyi kolayca ölçün: şeffaf, opak, aynasal, dağınık, cilalı, pürüzlü vb. NANOVEA Taşınabilir Profilometrelerin 2D ve 2D yetenekleri, onları hem laboratuvarda hem de sahada tam kapsamlı kaynak yüzeyi muayenesi için ideal cihazlar haline getirir.

ÖLÇÜM HEDEFI

Bu uygulamada, NANOVEA JR25 Taşınabilir Profilleyici, bir kaynağın yüzey pürüzlülüğünü, şeklini ve hacmini ve ayrıca çevresindeki alanı ölçmek için kullanılır. Bu bilgiler, kaynağın ve kaynak işleminin kalitesini doğru bir şekilde araştırmak için kritik bilgiler sağlayabilir.

NANOVEA

JR25

TEST SONUÇLARI

Aşağıdaki görüntü, kaynağın ve çevresindeki alanın tam 3D görünümünü ve yalnızca kaynağın yüzey parametrelerini göstermektedir. 2D kesit profili aşağıda gösterilmiştir.

örneklem

Yukarıdaki 2D kesit profili 3D'den çıkarıldığında, kaynağın boyutsal bilgileri aşağıda hesaplanır. Aşağıda sadece kaynak için yüzey alanı ve malzeme hacmi hesaplanmıştır.

 DELİKZİRVE
YÜZEY1.01 mm214.0 mm2
HACİM8.799e-5 mm323,27 mm3
MAKSIMUM DERINLIK/YÜKSEKLIK0,0276 mm0,6195 mm
ORTALAMA DERINLIK/YÜKSEKLIK 0.004024 mm 0,2298 mm

SONUÇ

Bu uygulamada, NANOVEA 3D Temassız Profilleyicinin bir kaynağın ve çevresindeki yüzey alanının kritik özelliklerini nasıl hassas bir şekilde karakterize edebileceğini gösterdik. Pürüzlülük, boyutlar ve hacimden, kalite ve tekrarlanabilirlik için nicel bir yöntem belirlenebilir ve / veya daha fazla araştırılabilir. Bu uygulama notundaki örnek gibi örnek kaynaklar, kurum içi veya saha testleri için standart bir masa üstü veya taşınabilir NANOVEA Profilleyici ile kolayca analiz edilebilir

Endüstriyel Kaplamalar Çizilme ve Aşınma Değerlendirmesi

ENDÜSTRİYEL KAPLAMA

TRIBOMETRE KULLANARAK ÇIZIK VE AŞINMA DEĞERLENDIRMESI

Tarafından hazırlanmıştır

DUANJIE LI, PhD & ANDREA HERRMANN

GİRİŞ

Akrilik üretan boya, zemin boyası, oto boyası ve diğerleri gibi çeşitli endüstriyel uygulamalarda yaygın olarak kullanılan hızlı kuruyan bir koruyucu kaplama türüdür. Zemin boyası olarak kullanıldığında, yürüyüş yolları, bordürler ve otoparklar gibi yoğun yaya ve lastik tekerlek trafiği olan alanlara hizmet edebilir.

KALİTE KONTROL İÇİN ÇİZİK VE AŞINMA TESTLERİNİN ÖNEMİ

Geleneksel olarak, ASTM D4060 standardına göre akrilik üretan zemin boyasının aşınma direncini değerlendirmek için Taber aşınma testleri gerçekleştirilmiştir. Ancak, standartta belirtildiği gibi, "Bazı malzemeler için, Taber Aşındırıcı kullanılarak yapılan aşınma testleri, test sırasında tekerleğin aşındırıcı özelliklerindeki değişiklikler nedeniyle değişkenliğe maruz kalabilir. "1 Bu, test sonuçlarının tekrarlanabilirliğinin zayıf olmasına ve farklı laboratuvarlardan bildirilen değerlerin karşılaştırılmasında zorluklara neden olabilir. Ayrıca, Taber aşınma testlerinde, aşınma direnci belirli sayıda aşınma döngüsünde ağırlık kaybı olarak hesaplanır. Bununla birlikte, akrilik üretan zemin boyalarının önerilen kuru film kalınlığı 37,5-50 μm2'dir.

Taber Abraser tarafından gerçekleştirilen agresif aşındırma işlemi akrilik üretan kaplamayı hızla aşındırabilir ve alt tabakada kütle kaybı yaratarak boya ağırlık kaybının hesaplanmasında önemli hatalara yol açabilir. Aşındırma testi sırasında boyaya aşındırıcı partiküllerin implantasyonu da hatalara katkıda bulunur. Bu nedenle, boyanın tekrarlanabilir aşınma değerlendirmesini sağlamak için iyi kontrol edilen ölçülebilir ve güvenilir bir ölçüm çok önemlidir. Buna ek olarak çizik testi kullanıcıların gerçek hayattaki uygulamalarda erken yapıştırıcı / tutkal arızalarını tespit etmelerini sağlar.

ÖLÇÜM HEDEFI

Bu çalışmada NANOVEA'nın Tribometreler ve Mekanik Test Cihazları Endüstriyel kaplamaların değerlendirilmesi ve kalite kontrolü için idealdir.

Farklı son katlara sahip akrilik üretan zemin boyalarının aşınma süreci, NANOVEA Tribometre kullanılarak kontrollü ve izlenebilir bir şekilde simüle edilmiştir. Mikro çizik testi, boyada yapışkan veya yapışkan arızasına neden olmak için gereken yükü ölçmek için kullanılır.

NANOVEA T100

Kompakt Pnömatik Tribometre

NANOVEA PB1000

Geniş Platform Mekanik Test Cihazı

TEST PROSEDÜRÜ

Bu çalışma, dayanıklılığı arttırmak amacıyla katkı karışımlarında küçük bir değişiklikle aynı formüle sahip aynı astar (taban kat) ve farklı son katlara sahip ticari olarak temin edilebilen dört su bazlı akrilik zemin kaplamasını değerlendirmektedir. Bu dört kaplama A, B, C ve D Örnekleri olarak tanımlanmıştır.

AŞINMA TESTİ

NANOVEA Tribometre, örneğin sürtünme katsayısı, COF ve aşınma direnci gibi tribolojik davranışı değerlendirmek için uygulandı. Test edilen boyalara bir SS440 bilye ucu (6 mm çap, Sınıf 100) uygulandı. COF yerinde kaydedildi. Aşınma oranı K, K=V/(F×s)=A/(F×n) formülü kullanılarak değerlendirildi; burada V aşınmış hacim, F normal yük, s kayma mesafesi, A ise aşınma izinin kesit alanı ve n, devir sayısıdır. Yüzey pürüzlülüğü ve aşınma izi profilleri NANOVEA tarafından değerlendirildi Optik Profilometreve aşınma izi morfolojisi optik mikroskop kullanılarak incelenmiştir.

AŞINMA TESTI PARAMETRELERI

NORMAL KUVVET

20 N

HIZ

15 m/dak

TEST SÜRESI

100, 150, 300 ve 800 döngü

ÇİZİK TESTİ

Rockwell C elmas uç (200 μm yarıçap) ile donatılmış NANOVEA Mekanik Test Cihazı, Mikro Çizik Test Cihazı Modu kullanılarak boya numuneleri üzerinde aşamalı yük çizik testleri gerçekleştirmek için kullanılmıştır. İki nihai yük kullanılmıştır: Boyanın astardan ayrılmasını incelemek için 5 N nihai yük ve astarın metal alt tabakalardan ayrılmasını incelemek için 35 N nihai yük. Sonuçların tekrarlanabilirliğini sağlamak için her numune üzerinde aynı test koşullarında üç test tekrarlanmıştır.

Tüm çizik uzunluklarının panoramik görüntüleri otomatik olarak oluşturuldu ve kritik arıza konumları sistem yazılımı tarafından uygulanan yüklerle ilişkilendirildi. Bu yazılım özelliği, kullanıcıların çizik testlerinden hemen sonra mikroskop altında kritik yükü belirlemek zorunda kalmak yerine, çizik izleri üzerinde istedikleri zaman analiz yapmalarını kolaylaştırmaktadır.

ÇIZIK TESTI PARAMETRELERI

YÜK TİPİİlerici
İLK YÜK0,01 mN
SON YÜK5 N / 35 N
YÜKLEME ORANI10 / 70 N/dak
ÇİZİK UZUNLUĞU3 mm
ÇİZME HIZI, dx/dt6,0 mm/dak
GIRINTI GEOMETRISI120º koni
GİRDİ MALZEMESİ (uç)Elmas
GIRINTI UCU YARIÇAPI200 μm

AŞINMA TESTI SONUÇLARI

Aşınmanın gelişimini izlemek için her bir numune üzerinde farklı devir sayılarında (100, 150, 300 ve 800 devir) dört adet pin-on-disk aşınma testi gerçekleştirilmiştir. Aşınma testi yapılmadan önce yüzey pürüzlülüğünü ölçmek için numunelerin yüzey morfolojisi NANOVEA 3D Temassız Profilleyici ile ölçülmüştür. Tüm numuneler, ŞEKİL 1'de gösterildiği gibi yaklaşık 1 μm'lik karşılaştırılabilir bir yüzey pürüzlülüğüne sahipti. COF, ŞEKİL 2'de gösterildiği gibi aşınma testleri sırasında in situ olarak kaydedilmiştir. ŞEKİL 4'te 100, 150, 300 ve 800 döngüden sonra aşınma izlerinin gelişimi ve ŞEKİL 3'te aşınma sürecinin farklı aşamalarında farklı numunelerin ortalama aşınma oranı özetlenmiştir.

 

Diğer üç numune için ~0,07 olan COF değeri ile karşılaştırıldığında, Numune A başlangıçta ~0,15 gibi çok daha yüksek bir COF sergilemekte, bu değer kademeli olarak artmakta ve 300 aşınma döngüsünden sonra ~0,3'te sabitlenmektedir. Bu kadar yüksek bir COF aşınma sürecini hızlandırır ve ŞEKİL 4'te gösterildiği gibi önemli miktarda boya döküntüsü oluşturur - Örnek A'nın son kat boyası ilk 100 devirde sökülmeye başlamıştır. ŞEKİL 3'te gösterildiği gibi, Örnek A ilk 300 devirde ~5 μm2/N ile en yüksek aşınma oranını sergilemekte, metal alt tabakanın daha iyi aşınma direnci nedeniyle bu oran ~3,5 μm2/N'ye hafifçe düşmektedir. Örnek C'nin üst kaplaması ŞEKİL 4'te gösterildiği gibi 150 aşınma döngüsünden sonra bozulmaya başlar ve bu durum ŞEKİL 2'deki COF artışıyla da gösterilir.

 

Karşılaştırıldığında, Örnek B ve Örnek D gelişmiş tribolojik özellikler göstermektedir. Örnek B tüm test boyunca düşük COF değerini korur - COF değeri ~0,05'ten ~0,1'e hafifçe yükselir. Böyle bir yağlama etkisi aşınma direncini önemli ölçüde artırır - son kat, 800 aşınma döngüsünden sonra alttaki astara hala üstün koruma sağlar. En düşük ortalama aşınma oranı 800 döngüde sadece ~0,77 μm2/N ile Örnek B için ölçülmüştür. Örnek D'nin üst kaplaması, ŞEKİL 2'de COF'nin ani artışıyla yansıtıldığı gibi 375 döngüden sonra delaminasyona başlar. Örnek D'nin ortalama aşınma oranı 800 döngüde ~1,1 μm2/N'dir.

 

Geleneksel Taber aşınma ölçümleriyle karşılaştırıldığında NANOVEA Tribometre, ticari zemin/otomotiv boyalarının tekrarlanabilir değerlendirmelerini ve kalite kontrolünü sağlayan iyi kontrollü ölçülebilir ve güvenilir aşınma değerlendirmeleri sağlar. Ayrıca, in situ COF ölçümlerinin kapasitesi, kullanıcıların bir aşınma sürecinin farklı aşamalarını COF'un evrimi ile ilişkilendirmesine olanak tanır; bu da çeşitli boya kaplamalarının aşınma mekanizması ve tribolojik özelliklerinin temel anlayışını geliştirmede kritik öneme sahiptir.

ŞEKİL 1: Boya örneklerinin 3D morfolojisi ve pürüzlülüğü.

ŞEKİL 2: Pin-on-disk testleri sırasında COF.

ŞEKİL 3: Farklı boyaların aşınma oranının evrimi.

ŞEKİL 4: Disk üzerinde pim testleri sırasında aşınma izlerinin evrimi.

ÇIZIK TESTI SONUÇLARI

ŞEKİL 5, Örnek A için çizik uzunluğunun bir fonksiyonu olarak normal kuvvet, sürtünme kuvveti ve gerçek derinlik grafiğini örnek olarak göstermektedir. Daha fazla bilgi sağlamak için isteğe bağlı bir akustik emisyon modülü takılabilir. Normal yük doğrusal olarak arttıkça, girinti ucu, gerçek derinliğin kademeli olarak artmasıyla yansıtıldığı gibi test edilen numuneye kademeli olarak batar. Sürtünme kuvveti ve gerçek derinlik eğrilerinin eğimlerindeki değişim, kaplama hatalarının oluşmaya başladığını gösteren sonuçlardan biri olarak kullanılabilir.

ŞEKİL 5: için çizik uzunluğunun bir fonksiyonu olarak normal kuvvet, sürtünme kuvveti ve gerçek derinlik Örnek A'nın maksimum 5 N yük ile çizik testi.

ŞEKİL 6 ve ŞEKİL 7 sırasıyla 5 N ve 35 N maksimum yük ile test edilen dört boya numunesinin tam çiziklerini göstermektedir. D numunesi astarı delamine etmek için 50 N'luk daha yüksek bir yük gerektirmiştir. 5 N nihai yükteki çizik testleri (ŞEKİL 6) üst boyanın kohezif/yapışkan hatasını değerlendirirken, 35 N'dakiler (ŞEKİL 7) astarın delaminasyonunu değerlendirmektedir. Mikrograflardaki oklar, üst kaplamanın veya astarın astardan veya alt tabakadan tamamen ayrılmaya başladığı noktayı göstermektedir. Kritik Yük, Lc olarak adlandırılan bu noktadaki yük, Tablo 1'de özetlendiği gibi boyanın kohezif veya yapışkan özelliklerini karşılaştırmak için kullanılır.

 

Boya Numunesi D'nin en iyi arayüzey yapışmasına sahip olduğu açıktır - boya delaminasyonunda 4,04 N ve astar delaminasyonunda 36,61 N ile en yüksek Lc değerlerini sergilemektedir. Örnek B ikinci en iyi çizilme direncini göstermektedir. Çizilme analizinden, boya formülünün optimizasyonunun mekanik davranışlar veya daha spesifik olarak akrilik zemin boyalarının çizilme direnci ve yapışma özelliği için kritik öneme sahip olduğunu gösteriyoruz.

Tablo 1: Kritik yüklerin özeti.

ŞEKİL 6: Maksimum 5 N yük ile tam çizik mikrografları.

ŞEKİL 7: Maksimum 35 N yük ile tam çizik mikrografları.

SONUÇ

Geleneksel Taber aşınma ölçümleriyle karşılaştırıldığında, NANOVEA Mekanik Test Cihazı ve Tribometre, ticari zemin ve otomotiv kaplamalarının değerlendirilmesi ve kalite kontrolü için üstün araçlardır. Çizilme modundaki NANOVEA Mekanik Test Cihazı, bir kaplama sistemindeki yapışma / kohezyon sorunlarını tespit edebilir. NANOVEA Tribometre, boyaların aşınma direnci ve sürtünme katsayısı üzerinde iyi kontrollü ölçülebilir ve tekrarlanabilir tribolojik analiz sağlar.

 

Bu çalışmada test edilen su bazlı akrilik zemin kaplamaları üzerinde yapılan kapsamlı tribolojik ve mekanik analizlere dayanarak, Örnek B'nin en düşük COF ve aşınma oranına ve ikinci en iyi çizilme direncine sahip olduğunu, Örnek D'nin ise en iyi çizilme direncini ve ikinci en iyi aşınma direncini sergilediğini gösteriyoruz. Bu değerlendirme, farklı uygulama ortamlarındaki ihtiyaçları hedefleyen en iyi adayı değerlendirmemize ve seçmemize olanak sağlamaktadır.

 

NANOVEA Mekanik Test Cihazının Nano ve Mikro modüllerinin tümü ISO ve ASTM uyumlu girinti, çizik ve aşınma test cihazı modlarını içerir ve tek bir modülde boya değerlendirmesi için mevcut olan en geniş test yelpazesini sağlar. NANOVEA Tribometre, ISO ve ASTM uyumlu rotatif ve lineer modları kullanarak hassas ve tekrarlanabilir aşınma ve sürtünme testleri sunar ve isteğe bağlı yüksek sıcaklık aşınması, yağlama ve tribo-korozyon modülleri önceden entegre edilmiş tek bir sistemde mevcuttur. NANOVEA'nın eşsiz ürün yelpazesi, sertlik, Young modülü, kırılma tokluğu, yapışma, aşınma direnci ve diğerleri dahil olmak üzere ince veya kalın, yumuşak veya sert kaplamaların, filmlerin ve alt tabakaların tüm mekanik/tribolojik özelliklerini belirlemek için ideal bir çözümdür. Pürüzlülük gibi diğer yüzey ölçümlerine ek olarak çiziklerin ve aşınma izlerinin yüksek çözünürlüklü 3D görüntülemesi için isteğe bağlı NANOVEA Temassız Optik Profilleyiciler mevcuttur.

ŞIMDI, BAŞVURUNUZ HAKKINDA KONUŞALIM