{"id":8344,"date":"2020-05-11T05:07:45","date_gmt":"2020-05-11T05:07:45","guid":{"rendered":"https:\/\/nanovea.com\/?p=8344"},"modified":"2023-11-13T22:17:52","modified_gmt":"2023-11-13T22:17:52","slug":"%e6%8c%a1%e5%9c%88-%e6%bb%91%e5%8a%a8-%e7%a3%a8%e6%8d%9f-%e8%af%84%e4%bc%b0","status":"publish","type":"post","link":"https:\/\/nanovea.com\/zh\/block-on-ring-sliding-wear-evaluation\/","title":{"rendered":"\u73af-\u5757\u78e8\u635f\u6d4b\u8bd5"},"content":{"rendered":"<div data-elementor-type=\"wp-post\" data-elementor-id=\"8344\" class=\"elementor elementor-8344\" data-elementor-post-type=\"post\">\n\t\t\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-3a9803e6 elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"3a9803e6\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-13caf891\" data-id=\"13caf891\" data-element_type=\"column\" data-settings=\"{&quot;background_background&quot;:&quot;classic&quot;}\">\n\t\t\t<div class=\"elementor-widget-wrap\">\n\t\t\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-1a5e82a6 elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"1a5e82a6\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-77960ac2\" data-id=\"77960ac2\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-634241d9 elementor-widget elementor-widget-text-editor\" data-id=\"634241d9\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p style=\"text-align: left; color: #1b96cf; font-size: 24px; line-height: 30px;\"><strong><em>\u5757\u5bf9\u73af\u78e8\u635f\u8bc4\u4f30\u7684\u91cd\u8981\u6027<\/em><u><i><br \/><\/i><\/u><\/strong><\/p><div>\u6ed1\u52a8\u78e8\u635f\u662f\u6307\u4e24\u79cd\u6750\u6599\u5728\u8d1f\u8f7d\u4e0b\u7684\u63a5\u89e6\u533a\u76f8\u4e92\u6ed1\u52a8\u800c\u5bfc\u81f4\u7684\u6750\u6599\u9010\u6e10\u635f\u5931\u3002\u5b83\u4e0d\u53ef\u907f\u514d\u5730\u53d1\u751f\u5728\u673a\u5668\u548c\u53d1\u52a8\u673a\u8fd0\u884c\u7684\u5404\u79cd\u884c\u4e1a\u4e2d\uff0c\u5305\u62ec\u6c7d\u8f66\u3001\u822a\u7a7a\u822a\u5929\u3001\u77f3\u6cb9\u548c\u5929\u7136\u6c14\u4ee5\u53ca\u8bb8\u591a\u5176\u4ed6\u884c\u4e1a\u3002\u8fd9\u79cd\u6ed1\u52a8\u8fd0\u52a8\u9020\u6210\u4e25\u91cd\u7684\u673a\u68b0\u78e8\u635f\u548c\u8868\u9762\u7684\u6750\u6599\u8f6c\u79fb\uff0c\u53ef\u80fd\u5bfc\u81f4\u751f\u4ea7\u6548\u7387\u964d\u4f4e\uff0c\u673a\u5668\u6027\u80fd\u4e0b\u964d\uff0c\u751a\u81f3\u635f\u574f\u673a\u5668\u3002<\/div><div>\u00a0<\/div><p>\u00a0<\/p><div>\u6ed1\u52a8\u78e8\u635f\u5f80\u5f80\u6d89\u53ca\u63a5\u89e6\u8868\u9762\u53d1\u751f\u7684\u590d\u6742\u78e8\u635f\u673a\u5236\uff0c\u5982\u7c98\u7740\u78e8\u635f\u3001\u4e8c\u4f53\u78e8\u635f\u3001\u4e09\u4f53\u78e8\u635f\u548c\u75b2\u52b3\u78e8\u635f\u3002\u6750\u6599\u7684\u78e8\u635f\u884c\u4e3a\u53d7\u6b63\u5e38\u8f7d\u8377\u3001\u901f\u5ea6\u3001\u8150\u8680\u548c\u6da6\u6ed1\u7b49\u5de5\u4f5c\u73af\u5883\u7684\u663e\u7740\u5f71\u54cd\u3002\u591a\u624d\u591a\u827a <a href=\"https:\/\/nanovea.com\/tribometers\/\">\u6469\u64e6\u4eea <\/a>\u53ef\u4ee5\u6a21\u62df\u4e0d\u540c\u7684\u5b9e\u9645\u5de5\u4f5c\u6761\u4ef6\u5c06\u662f\u78e8\u635f\u8bc4\u4f30\u7684\u7406\u60f3\u9009\u62e9\u3002<br \/>\u73af\u5757 (ASTM G77) \u6d4b\u8bd5\u662f\u4e00\u79cd\u5e7f\u6cdb\u4f7f\u7528\u7684\u6280\u672f\uff0c\u53ef\u8bc4\u4f30\u6750\u6599\u5728\u4e0d\u540c\u6a21\u62df\u6761\u4ef6\u4e0b\u7684\u6ed1\u52a8\u78e8\u635f\u884c\u4e3a\uff0c\u4e3a\u7279\u5b9a\u6469\u64e6\u5b66\u5e94\u7528\u63d0\u4f9b\u53ef\u9760\u7684\u6750\u6599\u5bf9\u6392\u540d\u3002<\/div><div>\u00a0<\/div><div>\u00a0<\/div><p>\u00a0<\/p><p style=\"text-align: left; color: #1b96cf; font-size: 24px; line-height: 30px;\"><strong><em>\u6d4b\u91cf\u76ee\u6807<\/em><u><i><br \/><\/i><\/u><\/strong><\/p><p>\u5728\u8fd9\u4e2a\u5e94\u7528\u4e2d\uff0cNanovea\u673a\u68b0\u6d4b\u8bd5\u4eea\u6d4b\u91cf\u4e0d\u9508\u94a2SS304\u548c\u94ddAl6061\u91d1\u5c5e\u5408\u91d1\u6837\u54c1\u7684YS\u548cUTS\u3002\u6837\u54c1\u7684YS\u548cUTS\u503c\u662f\u516c\u8ba4\u7684\uff0c\u8fd9\u8868\u660eNanovea\u7684\u538b\u75d5\u65b9\u6cd5\u662f\u53ef\u9760\u7684\u3002<\/p><p>\u00a0<\/p><div style=\"text-align: center;\"><a href=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/05\/Figure-1.png\"><img fetchpriority=\"high\" decoding=\"async\" class=\"alignnone size-full wp-image-8348\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/05\/Figure-1.png\" alt=\"\" width=\"648\" height=\"408\" \/><\/a><\/div><p>Nanovea \u7684\u6469\u64e6\u78e8\u635f\u8bd5\u9a8c\u673a\u4f7f\u7528 Block-on-Ring \u6a21\u5757\u8bc4\u4f30\u4e86 S-10 \u73af\u4e0a H-30 \u5757\u7684\u6ed1\u52a8\u78e8\u635f\u884c\u4e3a\u3002 H-30 \u5757\u7531\u786c\u5ea6\u4e3a 30HRC \u7684 01 \u5de5\u5177\u94a2\u5236\u6210\uff0c\u800c S-10 \u73af\u7531\u8868\u9762\u786c\u5ea6\u4e3a 58 \u81f3 63 HRC \u7684 4620 \u578b\u94a2\u5236\u6210\uff0c\u73af\u76f4\u5f84\u7ea6\u4e3a 34.98 \u6beb\u7c73\u3002\u5728\u5e72\u71e5\u548c\u6da6\u6ed1\u7684\u73af\u5883\u4e2d\u8fdb\u884c\u5757\u73af\u6d4b\u8bd5\uff0c\u4ee5\u7814\u7a76\u5bf9\u78e8\u635f\u884c\u4e3a\u7684\u5f71\u54cd\u3002\u6da6\u6ed1\u6d4b\u8bd5\u662f\u5728 USP \u91cd\u77ff\u7269\u6cb9\u4e2d\u8fdb\u884c\u7684\u3002\u4f7f\u7528 Nanovea \u7684\u78e8\u635f\u8f68\u8ff9\u8fdb\u884c\u68c0\u67e5 <a href=\"https:\/\/nanovea.com\/profilometers\/\">3D\u975e\u63a5\u89e6\u5f0f\u8f6e\u5ed3\u4eea<\/a>\u3002\u6d4b\u8bd5\u53c2\u6570\u603b\u7ed3\u4e8e\u88681\u4e2d\u3002\u78e8\u635f\u7387\uff08K\uff09\u91c7\u7528\u516c\u5f0fK=V\/\uff08F\u00d7s\uff09\u8bc4\u4f30\uff0c\u5176\u4e2dV\u4e3a\u78e8\u635f\u4f53\u79ef\uff0cF\u4e3a\u6cd5\u5411\u8f7d\u8377\uff0cs\u4e3a\u6ed1\u52a8\u8ddd\u79bb\u3002<\/p><p>\u00a0<\/p><div style=\"text-align: center;\"><a href=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/05\/Table-1.png\"><img decoding=\"async\" class=\"alignnone size-full wp-image-8349\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/05\/Table-1.png\" alt=\"\" width=\"450\" height=\"106\" \/><\/a><\/div><p>\u00a0<\/p><p style=\"text-align: left; color: #1b96cf; font-size: 24px; line-height: 30px;\"><strong><em>\u7ed3\u679c\u548c\u8ba8\u8bba<\/em><u><i><br \/><\/i><\/u><\/strong><\/p><p style=\"margin: 0in; margin-bottom: .0001pt;\"><span style=\"font-family: 'Arial',sans-serif;\">\u56fe 2 \u6bd4\u8f83\u4e86\u5e72\u71e5\u548c\u6da6\u6ed1\u73af\u5883\u4e0b\u73af\u5757\u6d4b\u8bd5\u7684\u6469\u64e6\u7cfb\u6570 (COF)\u3002\u8be5\u5757\u5728\u5e72\u71e5\u73af\u5883\u4e2d\u7684\u6469\u64e6\u529b\u660e\u663e\u5927\u4e8e\u6da6\u6ed1\u73af\u5883\u4e2d\u7684\u6469\u64e6\u529b\u3002 COF<br \/>\u5728\u524d 50 \u8f6c\u7684\u78e8\u5408\u671f\u95f4\uff0cCOF \u4f1a\u6ce2\u52a8\uff0c\u5e76\u5728\u5176\u4f59 200 \u8f6c\u78e8\u635f\u6d4b\u8bd5\u4e2d\u8fbe\u5230\u7ea6 0.8 \u7684\u6052\u5b9a COF\u3002\u76f8\u6bd4\u4e4b\u4e0b\uff0c\u5728 USP \u91cd\u77ff\u7269\u6cb9\u6da6\u6ed1\u4e2d\u8fdb\u884c\u7684\u73af\u5757\u6d4b\u8bd5\u5728\u6574\u4e2a 500,000 \u8f6c\u78e8\u635f\u6d4b\u8bd5\u4e2d\u59cb\u7ec8\u8868\u73b0\u51fa 0.09 \u7684\u4f4e COF\u3002\u8be5\u6da6\u6ed1\u5242\u53ef\u5c06\u8868\u9762\u4e4b\u95f4\u7684\u6469\u64e6\u7cfb\u6570\u663e\u7740\u964d\u4f4e\u7ea6 90 \u500d\u3002<\/span><\/p><p style=\"margin: 0in; margin-bottom: .0001pt;\">\u00a0<\/p><p>\u56fe3\u548c\u56fe4\u663e\u793a\u4e86\u5e72\u78e8\u635f\u548c\u6da6\u6ed1\u78e8\u635f\u8bd5\u9a8c\u540e\u5757\u4e0a\u78e8\u635f\u75a4\u75d5\u7684\u5149\u5b66\u56fe\u50cf\u548c\u622a\u97622D\u8f6e\u5ed3\u3002\u78e8\u635f\u8f68\u8ff9\u91cf\u548c\u78e8\u635f\u7387\u5982\u88682\u6240\u793a\u3002\u5728\u8f83\u4f4e\u8f6c\u901f72 rpm\u3001200\u8f6c\u7684\u5e72\u78e8\u635f\u8bd5\u9a8c\u4e0b\uff0c\u94a2\u5757\u8868\u73b0\u51fa9.45 mm\u02d9\u7684\u5927\u78e8\u635f\u75a4\u75d5\u4f53\u79ef\u3002\u76f8\u6bd4\u4e4b\u4e0b\uff0c\u5728\u77ff\u7269\u6cb9\u6da6\u6ed1\u5242\u4e2d\u4ee5197\u8f6c\/\u5206\u949f\u300150\u8f6c\u7684\u66f4\u9ad8\u8f6c\u901f\u8fdb\u884c\u7684\u78e8\u635f\u8bd5\u9a8c\uff0c\u4ea7\u751f\u7684\u78e8\u635f\u8f68\u8ff9\u4f53\u79ef\u5f88\u5c0f\uff0c\u4e3a0.03 mm\u02d9\u3002<\/p><p>\u00a0<\/p><p style=\"margin: 0in; margin-bottom: .0001pt;\"><span style=\"font-family: 'Arial',sans-serif;\"><br \/>\u00ffgure 3\u4e2d\u7684\u56fe\u50cf\u663e\u793a\u5728\u5e72\u71e5\u6761\u4ef6\u4e0b\u7684\u8bd5\u9a8c\u4e2d\u53d1\u751f\u4e86\u4e25\u91cd\u78e8\u635f\uff0c\u800c\u6da6\u6ed1\u78e8\u635f\u8bd5\u9a8c\u4e2d\u5219\u53d1\u751f\u4e86\u8f7b\u5fae\u78e8\u635f\u3002\u5e72\u78e8\u635f\u8bd5\u9a8c\u8fc7\u7a0b\u4e2d\u4ea7\u751f\u7684\u9ad8\u6e29\u548c\u5f3a\u70c8\u632f\u52a8\u4fc3\u8fdb\u4e86\u91d1\u5c5e\u788e\u7247\u7684\u6c27\u5316\uff0c\u5bfc\u81f4\u4e25\u91cd\u7684\u4e09\u4f53\u78e8\u635f\u3002\u5728\u6da6\u6ed1\u6d4b\u8bd5\u4e2d\uff0c\u77ff\u7269\u6cb9\u51cf\u5c11\u6469\u64e6\uff0c\u51b7\u5374\u63a5\u89e6\u8868\u9762\uff0c\u5e76\u5c06\u78e8\u635f\u8fc7\u7a0b\u4e2d\u4ea7\u751f\u7684\u78e8\u6599\u788e\u7247\u8fd0\u8f93\u6389\u3002\u8fd9\u5bfc\u81f4\u78e8\u635f\u7387\u964d\u4f4e\u4e86signi\u00ffcant ~8\u00d710\u3002\u5728\u4e0d\u540c\u7684\u73af\u5883\u4e2d\u8010\u78e8\u6027\u7684\u8fd9\u79cd\u5de8\u5927\u5dee\u5f02\u8868\u660e\u4e86\u5728\u5b9e\u9645\u4f7f\u7528\u6761\u4ef6\u4e0b\u8fdb\u884c\u9002\u5f53\u6ed1\u52a8\u78e8\u635f\u6a21\u62df\u7684\u91cd\u8981\u6027\u3002<\/span><\/p><p>\u00a0<\/p><p style=\"margin: 0in; margin-bottom: .0001pt;\"><span style=\"font-family: 'Arial',sans-serif;\"><br \/>\u5f53\u8bd5\u9a8c\u6761\u4ef6\u53d1\u751f\u5fae\u5c0f\u53d8\u5316\u65f6\uff0c\u78e8\u635f\u884c\u4e3a\u53ef\u80fd\u53d1\u751f\u5267\u70c8\u53d8\u5316\u3002Nanovea\u7684\u6469\u64e6\u8ba1\u7684\u591a\u529f\u80fd\u6027\u5141\u8bb8\u5728\u9ad8\u6e29\u3001\u6da6\u6ed1\u548c\u6469\u64e6\u8150\u8680\u6761\u4ef6\u4e0b\u8fdb\u884c\u78e8\u635f\u6d4b\u91cf\u3002\u7cbe\u786e\u7684\u901f\u5ea6\u548c\u4f4d\u7f6e\u63a7\u5236\u7684\u5148\u8fdb\u7535\u673a\u4f7f\u78e8\u635f\u6d4b\u8bd5\u6267\u884c\u7684\u901f\u5ea6\u4ece0.001\u52305000 rpm\uff0c\u4f7f\u5176\u6210\u4e3a\u7814\u7a76\/\u6d4b\u8bd5\u5b9e\u9a8c\u5ba4\u7684\u7406\u60f3\u5de5\u5177\uff0c\u4ee5\u8c03\u67e5\u78e8\u635f\u5728\u4e0d\u540c\u7684\u6469\u64e6\u5b66\u6761\u4ef6\u3002<\/span><\/p><p style=\"margin: 0in; margin-bottom: .0001pt;\">\u00a0<\/p><p>\u7528Nanovea\u7684\u975e\u63a5\u89e6\u5149\u5b66pro\u00fflometer\u68c0\u6d4b\u6837\u54c1\u7684\u8868\u9762\u72b6\u51b5\u3002\u56fe5\u663e\u793a\u4e86\u78e8\u635f\u8bd5\u9a8c\u540e\u73af\u7684\u8868\u9762\u5f62\u8c8c\u3002\u4e3a\u4e86\u66f4\u597d\u5730\u5448\u73b0\u6ed1\u52a8\u78e8\u635f\u8fc7\u7a0b\u4e2d\u4ea7\u751f\u7684\u8868\u9762\u5f62\u8c8c\u548c\u7c97\u7cd9\u5ea6\uff0c\u53bb\u6389\u4e86\u5706\u67f1\u5f62\u3002Signi\u00ffcant\u5728200\u8f6c\u7684\u5e72\u78e8\u635f\u8bd5\u9a8c\u4e2d\uff0c\u7531\u4e8e\u4e09\u4f53\u78e8\u635f\u8fc7\u7a0b\u53d1\u751f\u4e86\u8868\u9762\u7c97\u7cd9\u5316\u3002\u5e72\u78e8\u635f\u8bd5\u9a8c\u540e\u7684\u5757\u4f53\u548c\u73af\u4f53\u7684\u7c97\u7cd9\u5ea6Ra\u5206\u522b\u4e3a14.1\u548c18.1 \u03bc m\uff0c\u800c\u5728\u8f83\u9ad8\u901f\u5ea6\u4e0b\u8fdb\u884c50\u4e07\u8f6c\u957f\u671f\u6da6\u6ed1\u78e8\u635f\u8bd5\u9a8c\u540e\u7684\u7c97\u7cd9\u5ea6Ra\u5206\u522b\u4e3a5.7\u548c9.1 \u03bc m\u3002\u8be5\u8bd5\u9a8c\u8bc1\u660e\u4e86\u6d3b\u585e\u73af-\u6c14\u7f38\u63a5\u89e6\u5904\u9002\u5f53\u6da6\u6ed1\u7684\u91cd\u8981\u6027\u3002\u4e25\u91cd\u7684\u78e8\u635f\u4f1a\u8fc5\u901f\u635f\u574f\u6ca1\u6709\u6da6\u6ed1\u7684\u63a5\u89e6\u9762\uff0c\u5bfc\u81f4\u4f7f\u7528\u8d28\u91cf\u4e0d\u53ef\u9006\u7684\u6076\u5316\uff0c\u751a\u81f3\u5bfc\u81f4\u53d1\u52a8\u673a\u635f\u574f\u3002<\/p><p>\u00a0<\/p><p style=\"margin: 0in; margin-bottom: .0001pt;\"><span style=\"font-family: 'Arial',sans-serif; color: #1c1e29;\">\u00a0<\/span><\/p><div style=\"text-align: center;\"><p><a href=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/05\/Figure-2-and-3.png\"><img decoding=\"async\" class=\"alignnone size-full wp-image-8350\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/05\/Figure-2-and-3.png\" alt=\"\" width=\"574\" height=\"847\" \/><\/a><\/p><p><a href=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/05\/Figure-4-and-Table-2.png\"><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-8351\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/05\/Figure-4-and-Table-2.png\" alt=\"\" width=\"671\" height=\"860\" \/><\/a><\/p><\/div><p style=\"text-align: left; color: #1b96cf; font-size: 24px; line-height: 30px;\"><strong><em>\u7ed3\u8bba<\/em><u><i><br \/><\/i><\/u><\/strong><\/p><div style=\"text-align: center;\"><a href=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/05\/Conclusion-Pic.png\"><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-8352\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/05\/Conclusion-Pic.png\" alt=\"\" width=\"699\" height=\"491\" \/><\/a><\/div><p>\u5728\u672c\u7814\u7a76\u4e2d\uff0c\u6211\u4eec\u5c55\u793a\u4e86\u5982\u4f55\u4f7f\u7528 Nanovea \u7684\u6469\u64e6\u8ba1\u6765\u8bc4\u4f30\u94a2\u91d1\u5c5e\u5bf9\u7684\u6ed1\u52a8\u78e8\u635f\u884c\u4e3a\uff0c\u5e76\u4f7f\u7528\u9075\u5faa ASTM G77 \u6807\u51c6\u7684\u73af\u4e0a\u5757\u6a21\u5757\u3002\u6da6\u6ed1\u5242\u5728\u6750\u6599\u5bf9\u7684\u78e8\u635f\u6027\u80fd\u4e2d\u8d77\u7740\u81f3\u5173\u91cd\u8981\u7684\u4f5c\u7528\u3002\u77ff\u7269\u6cb9\u53ef\u5c06 H-30 \u5757\u7684\u78e8\u635f\u7387\u964d\u4f4e\u7ea6 8\u00d710\u02c6 \u500d\uff0c\u5c06 COF \u964d\u4f4e\u7ea6 90 \u500d\u3002 Nanovea \u6469\u64e6\u8ba1\u7684\u591a\u529f\u80fd\u6027\u4f7f\u5176\u6210\u4e3a\u6d4b\u91cf\u5404\u79cd\u6da6\u6ed1\u3001\u9ad8\u6e29\u548c\u6469\u64e6\u8150\u8680\u6761\u4ef6\u4e0b\u78e8\u635f\u884c\u4e3a\u7684\u7406\u60f3\u5de5\u5177\u3002<\/p><p>Nanovea \u7684\u6469\u64e6\u8bd5\u9a8c\u673a\u4f7f\u7528\u7b26\u5408 ISO \u548c ASTM \u7684\u65cb\u8f6c\u548c\u7ebf\u6027\u6a21\u5f0f\u63d0\u4f9b\u7cbe\u786e\u4e14\u53ef\u91cd\u590d\u7684\u78e8\u635f\u548c\u6469\u64e6\u6d4b\u8bd5\uff0c\u5e76\u5728\u4e00\u4e2a\u9884\u96c6\u6210\u7cfb\u7edf\u4e2d\u63d0\u4f9b\u53ef\u9009\u7684\u9ad8\u6e29\u78e8\u635f\u3001\u6da6\u6ed1\u548c\u6469\u64e6\u8150\u8680\u6a21\u5757\u3002 Nanovea \u65e0\u4e0e\u4f26\u6bd4\u7684\u7cfb\u5217\u662f\u786e\u5b9a\u8584\u6216\u539a\u3001\u8f6f\u6216\u786c\u6d82\u5c42\u3001\u8584\u819c\u548c\u57fa\u6750\u7684\u5168\u65b9\u4f4d\u6469\u64e6\u5b66\u7279\u6027\u7684\u7406\u60f3\u89e3\u51b3\u65b9\u6848\u3002<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-d39e8a2 elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"d39e8a2\" data-element_type=\"section\" data-settings=\"{&quot;background_background&quot;:&quot;classic&quot;}\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-a5d0b1d\" data-id=\"a5d0b1d\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-1b82dad elementor-widget elementor-widget-heading\" data-id=\"1b82dad\" data-element_type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\"><b>\u73b0\u5728\uff0c\u8ba9\u6211\u4eec\u6765\u8c08\u8c08\u4f60\u7684\u7533\u8bf7<\/b><\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-414bcdf live-chat elementor-align-center elementor-widget elementor-widget-button\" data-id=\"414bcdf\" data-element_type=\"widget\" data-widget_type=\"button.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<div class=\"elementor-button-wrapper\">\n\t\t\t\t\t<a class=\"elementor-button elementor-button-link elementor-size-md\" href=\"https:\/\/nanovea.com\/contact\/live-chat\/\" id=\"live-chat\">\n\t\t\t\t\t\t<span class=\"elementor-button-content-wrapper\">\n\t\t\t\t\t\t\t\t\t<span class=\"elementor-button-text\">\u5b9e\u65f6\u804a\u5929<\/span>\n\t\t\t\t\t<\/span>\n\t\t\t\t\t<\/a>\n\t\t\t\t<\/div>\n\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<\/div>","protected":false},"excerpt":{"rendered":"<p>IMPORTANCE OF BLOCK-ON-RING WEAR EVALUATION Sliding wear is the progressive loss of material that results from two materials sliding against each other at the contact area under load. It occurs inevitably in a wide variety of industries where machines and engines are in operation, including automotive, aerospace, oil &amp; gas and many others. Such sliding [&hellip;]<\/p>\n","protected":false},"author":1,"featured_media":11684,"comment_status":"open","ping_status":"open","sticky":false,"template":"","format":"standard","meta":{"_exactmetrics_skip_tracking":false,"_exactmetrics_sitenote_active":false,"_exactmetrics_sitenote_note":"","_exactmetrics_sitenote_category":0,"footnotes":""},"categories":[7,374,349,351,353,355,335,336],"tags":[],"class_list":["post-8344","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-application-notes","category-block-on-ring-tribology","category-laboratory-testing","category-profilometry-roughness-finish","category-profilometry-texture-grain","category-profilometry-volume-area","category-profilometry-testing","category-tribology-testing"],"_links":{"self":[{"href":"https:\/\/nanovea.com\/zh\/wp-json\/wp\/v2\/posts\/8344","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/nanovea.com\/zh\/wp-json\/wp\/v2\/posts"}],"about":[{"href":"https:\/\/nanovea.com\/zh\/wp-json\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"https:\/\/nanovea.com\/zh\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/nanovea.com\/zh\/wp-json\/wp\/v2\/comments?post=8344"}],"version-history":[{"count":19,"href":"https:\/\/nanovea.com\/zh\/wp-json\/wp\/v2\/posts\/8344\/revisions"}],"predecessor-version":[{"id":23411,"href":"https:\/\/nanovea.com\/zh\/wp-json\/wp\/v2\/posts\/8344\/revisions\/23411"}],"wp:featuredmedia":[{"embeddable":true,"href":"https:\/\/nanovea.com\/zh\/wp-json\/wp\/v2\/media\/11684"}],"wp:attachment":[{"href":"https:\/\/nanovea.com\/zh\/wp-json\/wp\/v2\/media?parent=8344"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"https:\/\/nanovea.com\/zh\/wp-json\/wp\/v2\/categories?post=8344"},{"taxonomy":"post_tag","embeddable":true,"href":"https:\/\/nanovea.com\/zh\/wp-json\/wp\/v2\/tags?post=8344"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}