{"id":7821,"date":"2017-02-11T14:40:05","date_gmt":"2017-02-11T14:40:05","guid":{"rendered":"https:\/\/nanovea.com\/?p=7821"},"modified":"2023-06-08T16:10:38","modified_gmt":"2023-06-08T16:10:38","slug":"%e5%be%aa%e7%8e%af-%e7%ba%b3%e7%b1%b3%e5%8e%8b%e7%97%95-%e5%ba%94%e5%8a%9b-%e5%ba%94%e5%8f%98-%e6%b5%8b%e9%87%8f","status":"publish","type":"post","link":"https:\/\/nanovea.com\/zh\/cyclical-nanoindentation-stress-strain-measurement\/","title":{"rendered":"\u5faa\u73af\u7eb3\u7c73\u538b\u75d5\u5e94\u529b-\u5e94\u53d8\u6d4b\u91cf"},"content":{"rendered":"<div data-elementor-type=\"wp-post\" data-elementor-id=\"7821\" class=\"elementor elementor-7821\" data-elementor-post-type=\"post\">\n\t\t\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-ae03426 elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"ae03426\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-3076502\" data-id=\"3076502\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-204420a elementor-widget elementor-widget-text-editor\" data-id=\"204420a\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p>\u5faa\u73af\u7eb3\u7c73\u538b\u75d5\u5e94\u529b-\u5e94\u53d8\u6d4b\u91cf<\/p><p>\u4e86\u89e3\u66f4\u591a<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-50946b6 elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"50946b6\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-fc2fac0\" data-id=\"fc2fac0\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<section class=\"elementor-section elementor-inner-section elementor-element elementor-element-a4810fe elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"a4810fe\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-inner-column elementor-element elementor-element-c762b93\" data-id=\"c762b93\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-ff3ffd3 elementor-widget elementor-widget-spacer\" data-id=\"ff3ffd3\" data-element_type=\"widget\" data-widget_type=\"spacer.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t<div class=\"elementor-spacer\">\n\t\t\t<div class=\"elementor-spacer-inner\"><\/div>\n\t\t<\/div>\n\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-inner-column elementor-element elementor-element-4ec3aee\" data-id=\"4ec3aee\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-8aa6fc7 elementor-widget elementor-widget-html\" data-id=\"8aa6fc7\" data-element_type=\"widget\" data-widget_type=\"html.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<div><\/div>\r\n<a href=\"http:\/\/nanovea.com\/App-Notes\/nanostressstrain.pdf\"\" target=\"_blank\">\r\n<div class=\"product-features-icon-image-containter-brochure-button\">\r\n\r\n<img decoding=\"async\" class=\"alignright\" style=\"width: 200px;\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2020\/06\/DOWNLOAD-PDF-BUTTON-A-s.png\" \/>\r\n<div class=\"overlay-button\"><img decoding=\"async\" class=\"alignright\" style=\"width: 200px;\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2020\/06\/DOWNLOAD-PDF-BUTTON-B-s.png\" \/><\/div>\r\n<\/div>\r\n<\/a>\r\n<div>\u00a0<\/div>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-32038d4b elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"32038d4b\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-5df39811\" data-id=\"5df39811\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-22614488 elementor-widget elementor-widget-text-editor\" data-id=\"22614488\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p style=\"text-align: left; color: #1b96cf; font-size: 24px;\">\u7eb3\u7c73\u538b\u75d5\u7684\u91cd\u8981\u6027<strong><u><i><br \/><\/i><\/u><\/strong><\/p><p style=\"margin: 0in; margin-bottom: .0001pt;\"><span style=\"font-family: 'Arial',sans-serif;\">\u901a\u8fc7\u4ee5\u4e0b\u65b9\u5f0f\u83b7\u5f97\u7684\u8fde\u7eed\u521a\u5ea6\u6d4b\u91cf\uff08CSM\uff09 <a href=\"https:\/\/nanovea.com\/nano-indentation-tester\/\">\u7eb3\u7c73\u538b\u75d5<\/a> \u7528\u5fae\u521b\u7684\u65b9\u6cd5\u63ed\u793a\u6750\u6599\u7684\u5e94\u529b-\u5e94\u53d8\u5173\u7cfb\u3002\u4e0e\u4f20\u7edf\u7684\u62c9\u4f38\u6d4b\u8bd5\u65b9\u6cd5\u4e0d\u540c\uff0c\u7eb3\u7c73\u538b\u75d5\u63d0\u4f9b\u7eb3\u7c73\u7ea7\u7684\u5e94\u529b-\u5e94\u53d8\u6570\u636e\uff0c\u800c\u4e0d\u9700\u8981\u5927\u578b\u4eea\u5668\u3002\u5e94\u529b-\u5e94\u53d8\u66f2\u7ebf\u63d0\u4f9b\u4e86\u5173\u4e8e\u6837\u54c1\u5728\u627f\u53d7\u8d8a\u6765\u8d8a\u5927\u7684\u8f7d\u8377\u65f6\u5f39\u6027\u548c\u5851\u6027\u884c\u4e3a\u4e4b\u95f4\u7684\u9608\u503c\u7684\u5173\u952e\u4fe1\u606f\u3002CSM\u63d0\u4f9b\u4e86\u5728\u6ca1\u6709\u5371\u9669\u8bbe\u5907\u7684\u60c5\u51b5\u4e0b\u786e\u5b9a\u6750\u6599\u7684\u5c48\u670d\u5e94\u529b\u7684\u80fd\u529b\u3002<\/span><\/p><p style=\"margin: 0in; margin-bottom: .0001pt;\"><span style=\"font-family: 'Arial',sans-serif;\">\u00a0<\/span><\/p><p>\u7eb3\u7c73\u538b\u75d5\u63d0\u4f9b\u4e86\u4e00\u79cd\u53ef\u9760\u7684\u548c\u7528\u6237\u53cb\u597d\u7684\u65b9\u6cd5\u6765\u5feb\u901f\u8c03\u67e5\u5e94\u529b-\u5e94\u53d8\u6570\u636e\u3002\u6b64\u5916\uff0c\u5728\u7eb3\u7c73\u5c3a\u5ea6\u4e0a\u6d4b\u91cf\u5e94\u529b-\u5e94\u53d8\u884c\u4e3a\u4f7f\u7814\u7a76\u6750\u6599\u4e2d\u7684\u5c0f\u6d82\u5c42\u548c\u9897\u7c92\u7684\u91cd\u8981\u7279\u6027\u6210\u4e3a\u53ef\u80fd\uff0c\u56e0\u4e3a\u5b83\u4eec\u53d8\u5f97\u66f4\u52a0\u5148\u8fdb\u3002\u9664\u4e86\u786c\u5ea6\u3001\u5f39\u6027\u6a21\u91cf\u3001\u8815\u53d8\u3001\u65ad\u88c2\u97e7\u6027\u7b49\uff0c\u7eb3\u7c73\u538b\u75d5\u8fd8\u80fd\u63d0\u4f9b\u5f39\u6027\u6781\u9650\u548c\u5c48\u670d\u5f3a\u5ea6\u7684\u4fe1\u606f\uff0c\u4f7f\u5176\u6210\u4e3a\u4e00\u79cd\u591a\u529f\u80fd\u7684\u8ba1\u91cf\u4eea\u5668\u3002<\/p><p>\u5728\u8fd9\u9879\u7814\u7a76\u4e2d\uff0c\u7eb3\u7c73\u538b\u75d5\u63d0\u4f9b\u7684\u5e94\u529b-\u5e94\u53d8\u6570\u636e\u786e\u5b9a\u4e86\u6750\u6599\u7684\u5f39\u6027\u6781\u9650\uff0c\u540c\u65f6\u53ea\u8fdb\u5165\u4e861.2\u5fae\u7c73\u7684\u8868\u9762\u3002\u6211\u4eec\u4f7f\u7528CSM\u6765\u786e\u5b9a\u6750\u6599\u7684\u673a\u68b0\u6027\u80fd\u662f\u5982\u4f55\u968f\u7740\u538b\u5934\u8fdb\u5165\u8868\u9762\u7684\u6df1\u5ea6\u800c\u53d1\u5c55\u7684\u3002\u8fd9\u5728\u8584\u819c\u5e94\u7528\u4e2d\u7279\u522b\u6709\u7528\uff0c\u56e0\u4e3a\u5176\u7279\u6027\u53ef\u80fd\u53d6\u51b3\u4e8e\u6df1\u5ea6\u3002\u7eb3\u7c73\u538b\u75d5\u662f\u4e00\u79cd\u786e\u8ba4\u6d4b\u8bd5\u6837\u54c1\u4e2d\u6750\u6599\u7279\u6027\u7684\u5fae\u521b\u65b9\u6cd5\u3002<\/p><p>CSM\u8bd5\u9a8c\u5728\u6d4b\u91cf\u6750\u6599\u7279\u6027\u4e0e\u6df1\u5ea6\u7684\u5173\u7cfb\u65b9\u9762\u5f88\u6709\u7528\u3002\u5faa\u73af\u8bd5\u9a8c\u53ef\u4ee5\u5728\u6052\u5b9a\u8f7d\u8377\u4e0b\u8fdb\u884c\uff0c\u4ee5\u786e\u5b9a\u66f4\u590d\u6742\u7684\u6750\u6599\u7279\u6027\u3002\u8fd9\u5bf9\u4e8e\u7814\u7a76\u75b2\u52b3\u6216\u6d88\u9664\u5b54\u9699\u7387\u7684\u5f71\u54cd\u4ee5\u83b7\u5f97\u771f\u6b63\u7684\u5f39\u6027\u6a21\u91cf\u662f\u5f88\u6709\u7528\u7684\u3002<\/p><p style=\"text-align: left; color: #1b96cf; font-size: 24px;\">\u6d4b\u91cf\u76ee\u6807<\/p><p style=\"margin: 0in; margin-bottom: .0001pt;\"><span style=\"font-family: 'Arial',sans-serif;\">\u5728\u8fd9\u4e2a\u5e94\u7528\u4e2d\uff0cNanovea\u673a\u68b0\u6d4b\u8bd5\u4eea\u4f7f\u7528CSM\u6765\u7814\u7a76\u786c\u5ea6\u548c\u5f39\u6027\u6a21\u91cf\u4e0e\u6df1\u5ea6\u7684\u5173\u7cfb\u4ee5\u53ca\u6807\u51c6\u94a2\u6837\u54c1\u7684\u5e94\u529b-\u5e94\u53d8\u6570\u636e\u3002\u94a2\u88ab\u9009\u62e9\u4e3a\u5176\u666e\u904d\u8ba4\u53ef\u7684\u7279\u6027\uff0c\u4ee5\u663e\u793a\u7eb3\u7c73\u7ea7\u5e94\u529b-\u5e94\u53d8\u6570\u636e\u7684\u63a7\u5236\u548c\u51c6\u786e\u6027\u3002\u4e00\u4e2a\u534a\u5f84\u4e3a5\u5fae\u7c73\u7684\u7403\u5f62\u5c16\u7aef\u88ab\u7528\u6765\u8fbe\u5230\u8db3\u591f\u9ad8\u7684\u5e94\u529b\uff0c\u8d85\u8fc7\u94a2\u7684\u5f39\u6027\u6781\u9650\u3002<\/span><\/p><p style=\"margin: 0in; margin-bottom: .0001pt;\"><span style=\"font-family: 'Arial',sans-serif;\">\u00a0<\/span><\/p><div style=\"text-align: center;\"><a href=\"https:\/\/nanovea.com\/wp-content\/uploads\/2020\/02\/2-Measurement-picture.png\"><img fetchpriority=\"high\" decoding=\"async\" class=\"alignnone size-full wp-image-7913\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2020\/02\/2-Measurement-picture.png\" alt=\"\" width=\"896\" height=\"725\" \/><\/a><\/div><p style=\"text-align: left; color: #1b96cf; font-size: 24px;\">\u6d4b\u8bd5\u6761\u4ef6\u548c\u7a0b\u5e8f<strong><u><i><br \/><\/i><\/u><\/strong><\/p><p style=\"margin: 0in; margin-bottom: .0001pt;\"><span style=\"font-family: 'Arial',sans-serif; color: #1c1e29;\">\u4f7f\u7528\u4e86\u4ee5\u4e0b\u538b\u75d5\u53c2\u6570\u3002<\/span><\/p><div style=\"text-align: center;\"><a href=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/02\/Figure-1.png\"><img decoding=\"async\" class=\"size-full wp-image-7830 aligncenter\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/02\/Figure-1.png\" alt=\"\" width=\"565\" height=\"607\" \/><\/a><\/div><p><em><strong style=\"color: black;\">\u7ed3\u679c\u3002 <\/strong><\/em><\/p><div>\u00a0<\/div><p style=\"margin: 0in; margin-bottom: .0001pt;\"><span style=\"font-family: 'Arial',sans-serif; color: #1c1e29;\">\u632f\u8361\u8fc7\u7a0b\u4e2d\u8d1f\u8f7d\u7684\u589e\u52a0\u63d0\u4f9b\u4e86\u4ee5\u4e0b\u6df1\u5ea6\u4e0e\u8d1f\u8f7d\u7684\u66f2\u7ebf\u3002\u5728\u52a0\u8f7d\u8fc7\u7a0b\u4e2d\u8fdb\u884c\u4e86100\u591a\u6b21\u632f\u8361\uff0c\u4ee5\u627e\u5230\u538b\u5934\u7a7f\u900f\u6750\u6599\u65f6\u7684\u5e94\u529b-\u5e94\u53d8\u6570\u636e\u3002<\/span><\/p><p style=\"margin: 0in; margin-bottom: .0001pt;\"><span style=\"font-family: 'Arial',sans-serif; color: #1c1e29;\">\u00a0<\/span><\/p><p style=\"margin: 0in; margin-bottom: .0001pt;\"><a href=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/02\/figure-2.png\"><img decoding=\"async\" class=\"alignnone size-full wp-image-7836\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/02\/figure-2.png\" alt=\"\" width=\"1040\" height=\"596\" \/><\/a><\/p><p>\u6211\u4eec\u4ece\u6bcf\u4e2a\u5468\u671f\u83b7\u5f97\u7684\u4fe1\u606f\u4e2d\u786e\u5b9a\u5e94\u529b\u548c\u5e94\u53d8\u3002\u6bcf\u4e2a\u5468\u671f\u7684\u6700\u5927\u8f7d\u8377\u548c\u6df1\u5ea6\u4f7f\u6211\u4eec\u80fd\u591f\u8ba1\u7b97\u51fa\u6bcf\u4e2a\u5468\u671f\u65bd\u52a0\u5728\u6750\u6599\u4e0a\u7684\u6700\u5927\u5e94\u529b\u3002\u5e94\u53d8\u662f\u7531\u6bcf\u4e2a\u5468\u671f\u7684\u90e8\u5206\u5378\u8f7d\u540e\u7684\u6b8b\u7559\u6df1\u5ea6\u8ba1\u7b97\u51fa\u6765\u7684\u3002\u8fd9\u4f7f\u6211\u4eec\u53ef\u4ee5\u901a\u8fc7\u9664\u4ee5\u5c16\u7aef\u7684\u534a\u5f84\u6765\u8ba1\u7b97\u6b8b\u7559\u5370\u8bb0\u7684\u534a\u5f84\uff0c\u4ece\u800c\u5f97\u5230\u5e94\u53d8\u7cfb\u6570\u3002\u7ed8\u5236\u6750\u6599\u7684\u5e94\u529b\u4e0e\u5e94\u53d8\u7684\u5173\u7cfb\u56fe\u663e\u793a\u4e86\u5f39\u6027\u533a\u548c\u5851\u6027\u533a\u4ee5\u53ca\u76f8\u5e94\u7684\u5f39\u6027\u6781\u9650\u5e94\u529b\u3002\u6211\u4eec\u7684\u6d4b\u8bd5\u786e\u5b9a\u6750\u6599\u7684\u5f39\u6027\u533a\u548c\u5851\u6027\u533a\u4e4b\u95f4\u7684\u8fc7\u6e21\u662f\u57280.076\u5de6\u53f3\u7684\u5e94\u53d8\uff0c\u5f39\u6027\u6781\u9650\u4e3a1.45GPa\u3002<\/p><p><a href=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/02\/Figure-3-3.png\"><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-8312\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/02\/Figure-3-3.png\" alt=\"\" width=\"1442\" height=\"849\" \/><\/a><\/p><p>\u6bcf\u4e2a\u5468\u671f\u4f5c\u4e3a\u4e00\u4e2a\u5355\u4e00\u7684\u538b\u75d5\uff0c\u6240\u4ee5\u5f53\u6211\u4eec\u589e\u52a0\u8d1f\u8f7d\u65f6\uff0c\u6211\u4eec\u5728\u94a2\u4e2d\u7684\u4e0d\u540c\u63a7\u5236\u6df1\u5ea6\u8fdb\u884c\u6d4b\u8bd5\u3002\u56e0\u6b64\uff0c\u786c\u5ea6\u548c\u5f39\u6027\u6a21\u91cf\u4e0e\u6df1\u5ea6\u7684\u5173\u7cfb\u53ef\u4ee5\u76f4\u63a5\u4ece\u6bcf\u4e2a\u5468\u671f\u83b7\u5f97\u7684\u6570\u636e\u4e2d\u7ed8\u5236\u51fa\u6765\u3002<\/p><p><a href=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/02\/Figure-4-2.png\"><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-8311\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/02\/Figure-4-2.png\" alt=\"\" width=\"1119\" height=\"566\" \/><\/a><\/p><p>\u968f\u7740\u538b\u5934\u8fdb\u5165\u6750\u6599\uff0c\u6211\u4eec\u770b\u5230\u786c\u5ea6\u589e\u52a0\uff0c\u5f39\u6027\u6a21\u91cf\u51cf\u5c11\u3002<\/p><p style=\"text-align: left; color: #1b96cf; font-size: 24px;\">\u603b\u7ed3<\/p><p><a href=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/02\/TiNCoatedPunches_NanoShieldPVD_Thailand.jpg\"><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-7848\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/02\/TiNCoatedPunches_NanoShieldPVD_Thailand.jpg\" alt=\"\" width=\"1624\" height=\"801\" \/><\/a><\/p><p>\u6211\u4eec\u5df2\u7ecf\u8bc1\u660eNanovea\u673a\u68b0\u6d4b\u8bd5\u4eea\u63d0\u4f9b\u53ef\u9760\u7684\u5e94\u529b-\u5e94\u53d8\u6570\u636e\u3002\u4f7f\u7528\u5e26\u6709CSM\u538b\u75d5\u7684\u7403\u5f62\u5c16\u7aef\uff0c\u53ef\u4ee5\u5728\u589e\u52a0\u7684\u5e94\u529b\u4e0b\u8fdb\u884c\u6750\u6599\u6027\u80fd\u6d4b\u91cf\u3002\u8d1f\u8f7d\u548c\u538b\u5934\u534a\u5f84\u53ef\u4ee5\u6539\u53d8\uff0c\u4ee5\u4fbf\u5728\u53d7\u63a7\u6df1\u5ea6\u6d4b\u8bd5\u5404\u79cd\u6750\u6599\u3002Nanovea\u673a\u68b0\u6d4b\u8bd5\u4eea\u63d0\u4f9b\u8fd9\u4e9b\u538b\u75d5\u6d4b\u8bd5\uff0c\u4ece\u4e9amN\u8303\u56f4\u5230400N\u3002<\/p><p>\u00a0<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<\/div>","protected":false},"excerpt":{"rendered":"<p>\u5faa\u73af\u7eb3\u7c73\u538b\u75d5\u5e94\u529b-\u5e94\u53d8\u6d4b\u91cf \u4e86\u89e3\u66f4\u591a<\/p>","protected":false},"author":1,"featured_media":7845,"comment_status":"open","ping_status":"open","sticky":false,"template":"","format":"standard","meta":{"_exactmetrics_skip_tracking":false,"_exactmetrics_sitenote_active":false,"_exactmetrics_sitenote_note":"","_exactmetrics_sitenote_category":0,"footnotes":""},"categories":[7,367,344,349,337,1],"tags":[],"class_list":["post-7821","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-application-notes","category-indentation-stress-strain","category-indentation-yield-strength-fatigue","category-laboratory-testing","category-mechanical-testing","category-uncategorized"],"_links":{"self":[{"href":"https:\/\/nanovea.com\/zh\/wp-json\/wp\/v2\/posts\/7821","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/nanovea.com\/zh\/wp-json\/wp\/v2\/posts"}],"about":[{"href":"https:\/\/nanovea.com\/zh\/wp-json\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"https:\/\/nanovea.com\/zh\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/nanovea.com\/zh\/wp-json\/wp\/v2\/comments?post=7821"}],"version-history":[{"count":31,"href":"https:\/\/nanovea.com\/zh\/wp-json\/wp\/v2\/posts\/7821\/revisions"}],"predecessor-version":[{"id":22574,"href":"https:\/\/nanovea.com\/zh\/wp-json\/wp\/v2\/posts\/7821\/revisions\/22574"}],"wp:featuredmedia":[{"embeddable":true,"href":"https:\/\/nanovea.com\/zh\/wp-json\/wp\/v2\/media\/7845"}],"wp:attachment":[{"href":"https:\/\/nanovea.com\/zh\/wp-json\/wp\/v2\/media?parent=7821"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"https:\/\/nanovea.com\/zh\/wp-json\/wp\/v2\/categories?post=7821"},{"taxonomy":"post_tag","embeddable":true,"href":"https:\/\/nanovea.com\/zh\/wp-json\/wp\/v2\/tags?post=7821"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}