{"id":20021,"date":"2022-05-27T22:23:41","date_gmt":"2022-05-27T22:23:41","guid":{"rendered":"https:\/\/nanovea.com\/?p=20021"},"modified":"2024-10-08T16:52:33","modified_gmt":"2024-10-08T16:52:33","slug":"%e5%b7%a5%e4%b8%9a%e6%b6%82%e6%96%99-%e5%88%92%e7%97%95%e5%92%8c%e7%a3%a8%e6%8d%9f-%e8%af%84%e4%bc%b0","status":"publish","type":"post","link":"https:\/\/nanovea.com\/zh\/industrial-coatings-scratch-and-wear-evaluation\/","title":{"rendered":"\u5de5\u4e1a\u6d82\u6599\u7684\u5212\u75d5\u548c\u78e8\u635f\u8bc4\u4f30"},"content":{"rendered":"<div data-elementor-type=\"wp-post\" data-elementor-id=\"20021\" class=\"elementor elementor-20021\" data-elementor-post-type=\"post\">\n\t\t\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-7ec3d48 elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"7ec3d48\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-c477953\" data-id=\"c477953\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-cec2c6e elementor-widget elementor-widget-heading\" data-id=\"cec2c6e\" data-element_type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h1 class=\"elementor-heading-title elementor-size-default\">\u5de5\u4e1a\u6d82\u6599<\/h1>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-d107f9b elementor-widget elementor-widget-heading\" data-id=\"d107f9b\" data-element_type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\">\u4f7f\u7528\u6469\u64e6\u8bd5\u9a8c\u673a\u8fdb\u884c\u5212\u75d5\u548c\u78e8\u635f\u8bc4\u4f30<\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-73c118d elementor-widget elementor-widget-image\" data-id=\"73c118d\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img fetchpriority=\"high\" decoding=\"async\" width=\"768\" height=\"242\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2022\/05\/Industrial-Coatings-Evaluation.jpg\" class=\"attachment-medium_large size-medium_large wp-image-20025\" alt=\"\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-97cc106 elementor-widget elementor-widget-heading\" data-id=\"97cc106\" data-element_type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\">\u7f16\u5199\u8005<\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-95aa94e elementor-widget elementor-widget-heading\" data-id=\"95aa94e\" data-element_type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\">\u674e\u7aef\u6770\u535a\u58eb\u548c\u5b89\u5fb7\u70c8\u4e9a-\u8d6b\u5c14\u66fc\u535a\u58eb<\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-c14383d elementor-widget elementor-widget-spacer\" data-id=\"c14383d\" data-element_type=\"widget\" data-widget_type=\"spacer.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t<div class=\"elementor-spacer\">\n\t\t\t<div class=\"elementor-spacer-inner\"><\/div>\n\t\t<\/div>\n\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-753c1f3 elementor-section-content-middle elementor-reverse-mobile elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"753c1f3\" data-element_type=\"section\" data-settings=\"{&quot;background_background&quot;:&quot;classic&quot;}\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-top-column elementor-element elementor-element-f2074e4 elementor-hidden-phone\" data-id=\"f2074e4\" data-element_type=\"column\" data-settings=\"{&quot;background_background&quot;:&quot;classic&quot;}\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-c0f91f8 elementor-widget elementor-widget-spacer\" data-id=\"c0f91f8\" data-element_type=\"widget\" data-widget_type=\"spacer.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t<div class=\"elementor-spacer\">\n\t\t\t<div class=\"elementor-spacer-inner\"><\/div>\n\t\t<\/div>\n\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-top-column elementor-element elementor-element-b259d86\" data-id=\"b259d86\" data-element_type=\"column\" data-settings=\"{&quot;background_background&quot;:&quot;classic&quot;}\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-62f2a44 elementor-widget elementor-widget-heading\" data-id=\"62f2a44\" data-element_type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\">\u7b80\u4ecb<\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-9ab0009 elementor-widget elementor-widget-text-editor\" data-id=\"9ab0009\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p>\u4e19\u70ef\u9178\u805a\u6c28\u916f\u6f06\u662f\u4e00\u79cd\u5feb\u5e72\u4fdd\u62a4\u6d82\u6599\uff0c\u5e7f\u6cdb\u7528\u4e8e\u5404\u79cd\u5de5\u4e1a\u5e94\u7528\uff0c\u5982\u5730\u677f\u6f06\u3001\u6c7d\u8f66\u6f06\u7b49\u3002\u5f53\u4f5c\u4e3a\u5730\u576a\u6f06\u4f7f\u7528\u65f6\uff0c\u5b83\u53ef\u4ee5\u670d\u52a1\u4e8e\u4eba\u6d41\u548c\u80f6\u8f6e\u8f66\u6d41\u91cf\u5927\u7684\u5730\u65b9\uff0c\u5982\u4eba\u884c\u9053\u3001\u8def\u8fb9\u548c\u505c\u8f66\u573a\u3002<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-d440447 elementor-widget elementor-widget-heading\" data-id=\"d440447\" data-element_type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\">\u5212\u75d5\u548c\u78e8\u635f\u6d4b\u8bd5\u5bf9\u8d28\u91cf\u63a7\u5236\u7684\u91cd\u8981\u6027<\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-966ab4d elementor-widget elementor-widget-text-editor\" data-id=\"966ab4d\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p>\u4f20\u7edf\u4e0a\uff0c\u6839\u636eASTM D4060\u6807\u51c6\uff0c\u91c7\u7528Taber\u78e8\u635f\u8bd5\u9a8c\u6765\u8bc4\u4f30\u4e19\u70ef\u9178\u805a\u6c28\u916f\u5730\u576a\u6f06\u7684\u8010\u78e8\u6027\u3002\u7136\u800c\uff0c\u6b63\u5982\u6807\u51c6\u4e2d\u6240\u63d0\u5230\u7684\uff0c\"\u5bf9\u4e8e\u67d0\u4e9b\u6750\u6599\uff0c\u7531\u4e8e\u6d4b\u8bd5\u8fc7\u7a0b\u4e2d\u8f66\u8f6e\u7684\u78e8\u6599\u7279\u6027\u53d1\u751f\u53d8\u5316\uff0c\u4f7f\u7528Taber\u78e8\u6599\u78e8\u5177\u8fdb\u884c\u7684\u78e8\u635f\u6d4b\u8bd5\u53ef\u80fd\u4f1a\u53d1\u751f\u53d8\u5316\u3002\u201c1\u8fd9\u53ef\u80fd\u5bfc\u81f4\u68c0\u6d4b\u7ed3\u679c\u7684\u53ef\u91cd\u590d\u6027\u5dee\uff0c\u5e76\u9020\u6210\u6bd4\u8f83\u4e0d\u540c\u5b9e\u9a8c\u5ba4\u62a5\u544a\u7684\u503c\u7684\u56f0\u96be\u3002\u6b64\u5916\uff0c\u5728Taber\u78e8\u635f\u8bd5\u9a8c\u4e2d\uff0c\u8010\u78e8\u6027\u8ba1\u7b97\u4e3a\u5728\u6307\u5b9a\u6b21\u6570\u7684\u78e8\u635f\u5faa\u73af\u4e0b\u7684\u91cd\u91cf\u635f\u5931\u3002\u800c\u4e19\u70ef\u9178\u805a\u6c28\u916f\u5730\u576a\u6f06\u7684\u63a8\u8350\u5e72\u819c\u539a\u5ea6\u4e3a37.5 ~ 50 \u03bcm2\u3002<\/p><p>Taber Abraser\u7684\u4fb5\u8680\u6027\u78e8\u8680\u8fc7\u7a0b\u53ef\u4ee5\u8fc5\u901f\u78e8\u7a7f\u4e19\u70ef\u9178\u805a\u6c28\u916f\u6d82\u5c42\uff0c\u5e76\u9020\u6210\u57fa\u6750\u7684\u8d28\u91cf\u635f\u5931\uff0c\u4ece\u800c\u5bfc\u81f4\u6d82\u6599\u91cd\u91cf\u635f\u5931\u8ba1\u7b97\u7684\u5de8\u5927\u8bef\u5dee\u3002\u5728\u78e8\u8680\u8bd5\u9a8c\u8fc7\u7a0b\u4e2d\uff0c\u78e8\u6599\u9897\u7c92\u690d\u5165\u6d82\u6599\u4e2d\u4e5f\u4f1a\u9020\u6210\u8bef\u5dee\u3002\u56e0\u6b64\uff0c\u4e00\u4e2a\u63a7\u5236\u826f\u597d\u7684\u53ef\u91cf\u5316\u548c\u53ef\u9760\u7684\u6d4b\u91cf\u5bf9\u4e8e\u786e\u4fdd\u6d82\u6599\u7684\u53ef\u91cd\u590d\u6027\u78e8\u635f\u8bc4\u4f30\u81f3\u5173\u91cd\u8981\u3002\u6b64\u5916\uff0c\u8fd8\u6709 <a href=\"https:\/\/nanovea.com\/scratch-tester\/\">\u5212\u75d5\u6d4b\u8bd5<\/a> \u5141\u8bb8\u7528\u6237\u5728\u5b9e\u9645\u5e94\u7528\u4e2d\u68c0\u6d4b\u5230\u8fc7\u65e9\u7684\u7c98\u5408\u5242\/\u80f6\u7c98\u5242\u5931\u6548\u3002<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-bbe0c25 elementor-reverse-mobile elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"bbe0c25\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-5bda47b\" data-id=\"5bda47b\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-353eff9 elementor-widget elementor-widget-heading\" data-id=\"353eff9\" data-element_type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\">\u6d4b\u91cf\u76ee\u6807<\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-5556e11 elementor-widget elementor-widget-text-editor\" data-id=\"5556e11\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p>\u5728\u8fd9\u9879\u7814\u7a76\u4e2d\uff0c\u6211\u4eec\u5c55\u793a\u4e86 NANOVEA <a href=\"https:\/\/nanovea.com\/tribometers\/\">\u6469\u64e6\u8ba1 <\/a>\u548c <a href=\"https:\/\/nanovea.com\/mechanical-testers\/\">\u5fae\u7eb3\u7c73\u529b\u5b66\u6d4b\u8bd5\u7cfb\u7edf<\/a> \u662f\u5de5\u4e1a\u6d82\u6599\u8bc4\u4f30\u548c\u8d28\u91cf\u63a7\u5236\u7684\u7406\u60f3\u9009\u62e9\u3002<\/p>\n<p>\u4f7f\u7528NANOVEA\u6469\u64e6\u4eea\uff0c\u4ee5\u63a7\u5236\u548c\u76d1\u6d4b\u7684\u65b9\u5f0f\u6a21\u62df\u4e0d\u540c\u9762\u6f06\u7684\u4e19\u70ef\u9178\u805a\u6c28\u916f\u5730\u677f\u6f06\u7684\u78e8\u635f\u8fc7\u7a0b\u3002\u5fae\u91cf\u5212\u75d5\u6d4b\u8bd5\u88ab\u7528\u6765\u6d4b\u91cf\u5bfc\u81f4\u6d82\u6599\u5185\u805a\u6216\u7c98\u5408\u5931\u6548\u6240\u9700\u7684\u8d1f\u8377\u3002<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<section class=\"elementor-section elementor-inner-section elementor-element elementor-element-5986dd7 elementor-reverse-mobile elementor-section-full_width elementor-reverse-tablet elementor-section-height-default elementor-section-height-default\" data-id=\"5986dd7\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-extended\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-inner-column elementor-element elementor-element-a6b67e5\" data-id=\"a6b67e5\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-911a059 elementor-widget elementor-widget-image\" data-id=\"911a059\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<a href=\"https:\/\/nanovea.com\/instruments\/t100\/\">\n\t\t\t\t\t\t\t<img decoding=\"async\" width=\"763\" height=\"800\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2020\/12\/Nanovea-T100-Affordable-Tribometer.png\" class=\"elementor-animation-grow attachment-medium_large size-medium_large wp-image-9908\" alt=\"\u7d27\u51d1\u578b\u6c14\u52a8\u6469\u64e6\u4eeaT100\" \/>\t\t\t\t\t\t\t\t<\/a>\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-cf30732 elementor-widget elementor-widget-text-editor\" data-id=\"cf30732\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<span style=\"color: #000000;\">NANOVEA <\/span><span style=\"color: #1b96cf;\">T100<\/span>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-7429702 elementor-widget elementor-widget-text-editor\" data-id=\"7429702\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p style=\"text-align: center;\">\u7d27\u51d1\u578b\u6c14\u52a8\u6469\u64e6\u4eea<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-48491b2 elementor-align-center learn-more-about-instrument elementor-widget elementor-widget-button\" data-id=\"48491b2\" data-element_type=\"widget\" data-widget_type=\"button.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<div class=\"elementor-button-wrapper\">\n\t\t\t\t\t<a class=\"elementor-button elementor-button-link elementor-size-md\" href=\"https:\/\/nanovea.com\/instruments\/t100\/\" id=\"learn-more-about-instrument\">\n\t\t\t\t\t\t<span class=\"elementor-button-content-wrapper\">\n\t\t\t\t\t\t\t\t\t<span class=\"elementor-button-text\">\u4e86\u89e3\u66f4\u591a<\/span>\n\t\t\t\t\t<\/span>\n\t\t\t\t\t<\/a>\n\t\t\t\t<\/div>\n\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-inner-column elementor-element elementor-element-6a846d8\" data-id=\"6a846d8\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-3956283 elementor-widget elementor-widget-image\" data-id=\"3956283\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<a href=\"https:\/\/nanovea.com\/instruments\/pb1000\/\">\n\t\t\t\t\t\t\t<img decoding=\"async\" width=\"600\" height=\"595\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2022\/05\/NANOVEA-Mechanical-Tester-PB1000.png\" class=\"elementor-animation-grow attachment-medium_large size-medium_large wp-image-20051\" alt=\"\" \/>\t\t\t\t\t\t\t\t<\/a>\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-42860bf elementor-widget elementor-widget-text-editor\" data-id=\"42860bf\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p style=\"text-align: center;\"><span style=\"color: #000000;\">NANOVEA <\/span><span style=\"color: #1b96cf;\">PB1000<\/span><\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-1f4a14e elementor-widget elementor-widget-text-editor\" data-id=\"1f4a14e\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p style=\"text-align: center;\">\u5927\u578b\u5e73\u53f0\u673a\u68b0\u6d4b\u8bd5\u4eea<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-2c016cf elementor-align-center learn-more-about-instrument elementor-widget elementor-widget-button\" data-id=\"2c016cf\" data-element_type=\"widget\" data-widget_type=\"button.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<div class=\"elementor-button-wrapper\">\n\t\t\t\t\t<a class=\"elementor-button elementor-button-link elementor-size-md\" href=\"https:\/\/nanovea.com\/instruments\/pb1000\/\" id=\"learn-more-about-instrument\">\n\t\t\t\t\t\t<span class=\"elementor-button-content-wrapper\">\n\t\t\t\t\t\t\t\t\t<span class=\"elementor-button-text\">\u4e86\u89e3\u66f4\u591a<\/span>\n\t\t\t\t\t<\/span>\n\t\t\t\t\t<\/a>\n\t\t\t\t<\/div>\n\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-1979bac elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"1979bac\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-no\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-c969083\" data-id=\"c969083\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-9c67049 elementor-widget elementor-widget-heading\" data-id=\"9c67049\" data-element_type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\">\u6d4b\u8bd5\u7a0b\u5e8f<\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-1ad96b0 elementor-widget elementor-widget-text-editor\" data-id=\"1ad96b0\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p style=\"text-align: left;\">\u672c\u7814\u7a76\u8bc4\u4f30\u4e86\u56db\u79cd\u5e02\u552e\u7684\u6c34\u6027\u4e19\u70ef\u9178\u5730\u677f\u6d82\u6599\uff0c\u5b83\u4eec\u5177\u6709\u76f8\u540c\u7684\u5e95\u6f06\uff08\u57fa\u5e95\u6f06\uff09\u548c\u76f8\u540c\u914d\u65b9\u7684\u4e0d\u540c\u9762\u6f06\uff0c\u4e3a\u4e86\u63d0\u9ad8\u8010\u4e45\u6027\uff0c\u5728\u6dfb\u52a0\u5242\u7684\u6df7\u5408\u4e0a\u6709\u5c0f\u7684\u53d8\u5316\u3002\u8fd9\u56db\u79cd\u6d82\u6599\u88ab\u786e\u5b9a\u4e3a\u6837\u54c1A\u3001B\u3001C\u548cD\u3002<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-42252f7 elementor-widget elementor-widget-image\" data-id=\"42252f7\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img loading=\"lazy\" decoding=\"async\" width=\"1024\" height=\"436\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2022\/05\/Industrial-Paint-Tribology.jpg\" class=\"attachment-large size-large wp-image-20036\" alt=\"\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-3b1c09f elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"3b1c09f\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-top-column elementor-element elementor-element-c3e7d88\" data-id=\"c3e7d88\" data-element_type=\"column\" data-settings=\"{&quot;background_background&quot;:&quot;classic&quot;}\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-704243a elementor-widget elementor-widget-spacer\" data-id=\"704243a\" data-element_type=\"widget\" data-widget_type=\"spacer.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t<div class=\"elementor-spacer\">\n\t\t\t<div class=\"elementor-spacer-inner\"><\/div>\n\t\t<\/div>\n\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-top-column elementor-element elementor-element-f13c2c1\" data-id=\"f13c2c1\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-9e3708e elementor-widget elementor-widget-heading\" data-id=\"9e3708e\" data-element_type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\">\u78e8\u635f\u6d4b\u8bd5<\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-80398c0 elementor-widget elementor-widget-text-editor\" data-id=\"80398c0\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p style=\"text-align: left;\">NANOVEA \u6469\u64e6\u8ba1\u7528\u4e8e\u8bc4\u4f30\u6469\u64e6\u5b66\u884c\u4e3a\uff0c\u4f8b\u5982\u6469\u64e6\u7cfb\u6570\u3001COF \u548c\u8010\u78e8\u6027\u3002\u5c06 SS440 \u7403\u5934\uff08\u76f4\u5f84 6 \u6beb\u7c73\uff0c\u7b49\u7ea7 100\uff09\u5e94\u7528\u4e8e\u6d4b\u8bd5\u6d82\u6599\u3002 COF \u662f\u73b0\u573a\u8bb0\u5f55\u7684\u3002\u78e8\u635f\u7387K\u7684\u8ba1\u7b97\u516c\u5f0f\u4e3aK=V\/(F\u00d7s)=A\/(F\u00d7n)\uff0c\u5176\u4e2dV\u4e3a\u78e8\u635f\u4f53\u79ef\uff0cF\u4e3a\u6cd5\u5411\u8f7d\u8377\uff0cs\u4e3a\u6ed1\u52a8\u8ddd\u79bb\uff0cA\u4e3a\u78e8\u635f\u8f68\u8ff9\u7684\u6a2a\u622a\u9762\u79ef\uff0cn\u662f\u8f6c\u6570\u3002\u8868\u9762\u7c97\u7cd9\u5ea6\u548c\u78e8\u635f\u8f68\u8ff9\u8f6e\u5ed3\u7531 NANOVEA \u8bc4\u4f30 <a href=\"https:\/\/nanovea.com\/profilometers\/\">\u5149\u5b66\u8f6e\u5ed3\u4eea<\/a>\uff0c\u5e76\u4f7f\u7528\u5149\u5b66\u663e\u5fae\u955c\u68c0\u67e5\u78e8\u635f\u8f68\u8ff9\u5f62\u6001\u3002<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-df053de elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"df053de\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-no\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-bbe3fd5\" data-id=\"bbe3fd5\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-0c30aad elementor-widget elementor-widget-heading\" data-id=\"0c30aad\" data-element_type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\">\u78e8\u635f\u6d4b\u8bd5\u53c2\u6570<\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<section class=\"elementor-section elementor-inner-section elementor-element elementor-element-a158972 elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"a158972\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-25 elementor-inner-column elementor-element elementor-element-a588777\" data-id=\"a588777\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap\">\n\t\t\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t<div class=\"elementor-column elementor-col-25 elementor-inner-column elementor-element elementor-element-d32c57a\" data-id=\"d32c57a\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-c0aad96 elementor-widget elementor-widget-text-editor\" data-id=\"c0aad96\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p>\u5e38\u6001\u529b<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-bafa675 elementor-widget elementor-widget-text-editor\" data-id=\"bafa675\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p>20 N<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t<div class=\"elementor-column elementor-col-25 elementor-inner-column elementor-element elementor-element-ce3ce36\" data-id=\"ce3ce36\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-3049f88 elementor-widget elementor-widget-text-editor\" data-id=\"3049f88\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p>\u901f\u5ea6<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-a80a88a elementor-widget elementor-widget-text-editor\" data-id=\"a80a88a\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p>15\u7c73\/\u5206\u949f<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t<div class=\"elementor-column elementor-col-25 elementor-inner-column elementor-element elementor-element-86350c3\" data-id=\"86350c3\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap\">\n\t\t\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<div class=\"elementor-element elementor-element-6bafc22 elementor-widget elementor-widget-text-editor\" data-id=\"6bafc22\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p>\u6d4b\u8bd5\u65f6\u95f4<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-8f4e1b9 elementor-widget elementor-widget-text-editor\" data-id=\"8f4e1b9\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p>100\u3001150\u3001300\u548c800\u5468\u671f<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-575156f elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"575156f\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-top-column elementor-element elementor-element-a106cd2\" data-id=\"a106cd2\" data-element_type=\"column\" data-settings=\"{&quot;background_background&quot;:&quot;classic&quot;}\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-3aad899 elementor-widget elementor-widget-spacer\" data-id=\"3aad899\" data-element_type=\"widget\" data-widget_type=\"spacer.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t<div class=\"elementor-spacer\">\n\t\t\t<div class=\"elementor-spacer-inner\"><\/div>\n\t\t<\/div>\n\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-top-column elementor-element elementor-element-0387f33\" data-id=\"0387f33\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-1188445 elementor-widget elementor-widget-heading\" data-id=\"1188445\" data-element_type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\">\u5212\u75d5\u6d4b\u8bd5<\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-292fb67 elementor-widget elementor-widget-text-editor\" data-id=\"292fb67\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p style=\"text-align: left;\">\u914d\u5907\u4e86\u7f57\u514b\u97e6\u5c14C\u91d1\u521a\u77f3\u89e6\u63a7\u7b14(200 \u03bcm\u534a\u5f84)\u7684NANOVEA\u673a\u68b0\u6d4b\u8bd5\u4eea\u4f7f\u7528\u5fae\u522e\u64e6\u6d4b\u8bd5\u6a21\u5f0f\u5bf9\u6cb9\u6f06\u6837\u54c1\u8fdb\u884c\u6e10\u8fdb\u8d1f\u8f7d\u522e\u64e6\u6d4b\u8bd5\u3002\u4f7f\u7528\u4e86\u4e24\u79cd\u6700\u7ec8\u8d1f\u8f7d:5 N\u7684\u6700\u7ec8\u8d1f\u8f7d\u7528\u4e8e\u7814\u7a76\u5e95\u6f06\u4e0a\u7684\u6cb9\u6f06\u5206\u5c42\uff0c35 N\u7684\u6700\u7ec8\u8d1f\u8f7d\u7528\u4e8e\u7814\u7a76\u91d1\u5c5e\u57fa\u6750\u4e0a\u7684\u5e95\u6f06\u5206\u5c42\u3002\u5bf9\u6bcf\u4e2a\u6837\u54c1\u5728\u76f8\u540c\u7684\u6d4b\u8bd5\u6761\u4ef6\u4e0b\u91cd\u590d\u8fdb\u884c\u4e09\u6b21\u6d4b\u8bd5\uff0c\u4ee5\u786e\u4fdd\u7ed3\u679c\u7684\u53ef\u91cd\u590d\u6027\u3002<\/p><p style=\"text-align: left;\">\u6574\u4e2a\u5212\u75d5\u957f\u5ea6\u7684\u5168\u666f\u56fe\u50cf\u88ab\u81ea\u52a8\u751f\u6210\uff0c\u5b83\u4eec\u7684\u4e34\u754c\u5931\u6548\u4f4d\u7f6e\u88ab\u7cfb\u7edf\u8f6f\u4ef6\u4e0e\u65bd\u52a0\u7684\u8f7d\u8377\u76f8\u5173\u8054\u3002\u8fd9\u4e00\u8f6f\u4ef6\u529f\u80fd\u4fbf\u4e8e\u7528\u6237\u968f\u65f6\u5bf9\u5212\u75d5\u8fdb\u884c\u5206\u6790\uff0c\u800c\u4e0d\u662f\u5728\u5212\u75d5\u6d4b\u8bd5\u540e\u7acb\u5373\u5728\u663e\u5fae\u955c\u4e0b\u786e\u5b9a\u4e34\u754c\u8f7d\u8377\u3002<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-4f2abf8 elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"4f2abf8\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-no\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-ef25143\" data-id=\"ef25143\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-09aead5 elementor-widget elementor-widget-heading\" data-id=\"09aead5\" data-element_type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\">\u5212\u75d5\u6d4b\u8bd5\u53c2\u6570<\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-f48b766 elementor-widget elementor-widget-text-editor\" data-id=\"f48b766\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<table style=\"width: 100%;\"><tbody><tr><td style=\"text-align: left; width: 67.7419%;\"><em><strong>\u88c5\u8f7d\u7c7b\u578b<\/strong><\/em><\/td><td style=\"width: 29.912%; text-align: right;\"><em><strong>\u6e10\u8fdb\u7684<\/strong><\/em><\/td><\/tr><tr><td style=\"text-align: left; width: 67.7419%;\"><em><strong>\u521d\u59cb\u8d1f\u8f7d<\/strong><\/em><\/td><td style=\"width: 29.912%; text-align: right;\"><em><strong>0.01 mN<\/strong><\/em><\/td><\/tr><tr><td style=\"text-align: left; width: 67.7419%;\"><em><strong>\u7ec8\u6781\u88c5\u8f7d<\/strong><\/em><\/td><td style=\"width: 29.912%; text-align: right;\"><em><strong>5 N \/ 35 N<\/strong><\/em><\/td><\/tr><tr><td style=\"text-align: left; width: 67.7419%;\"><em><strong>\u88c5\u8f7d\u7387<\/strong><\/em><\/td><td style=\"width: 29.912%; text-align: right;\"><em><strong>10 \/ 70 N\/min<\/strong><\/em><\/td><\/tr><tr><td style=\"text-align: left; width: 67.7419%;\"><em><strong>\u5212\u75d5\u957f\u5ea6<\/strong><\/em><\/td><td style=\"width: 29.912%; text-align: right;\"><em><strong>3\u6beb\u7c73<\/strong><\/em><\/td><\/tr><tr><td style=\"text-align: left; width: 67.7419%;\"><em><strong>\u522e\u64e6\u901f\u5ea6\uff0cdx\/dt<\/strong><\/em><\/td><td style=\"width: 29.912%; text-align: right;\"><em><strong>6.0\u6beb\u7c73\/\u5206\u949f<\/strong><\/em><\/td><\/tr><tr><td style=\"text-align: left; width: 67.7419%;\"><em><strong>\u538b\u5934\u7684\u51e0\u4f55\u5f62\u72b6<\/strong><\/em><\/td><td style=\"width: 29.912%; text-align: right;\"><em><strong>120\u00ba\u9525\u4f53<\/strong><\/em><\/td><\/tr><tr><td style=\"text-align: left; width: 67.7419%;\"><em><strong>\u538b\u5370\u6750\u6599\uff08\u5c16\u7aef\uff09<\/strong><\/em><\/td><td style=\"width: 29.912%; text-align: right;\"><em><strong>\u94bb\u77f3<\/strong><\/em><\/td><\/tr><tr><td style=\"text-align: left; width: 67.7419%;\"><em><strong>\u538b\u5934\u534a\u5f84<\/strong><\/em><\/td><td style=\"width: 29.912%; text-align: right;\"><em><strong>200 \u03bcm<\/strong><\/em><\/td><\/tr><\/tbody><\/table>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-1fa8af8 elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"1fa8af8\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-no\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-5652dcb\" data-id=\"5652dcb\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-8896e58 elementor-widget elementor-widget-heading\" data-id=\"8896e58\" data-element_type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\">\u78e8\u635f\u6d4b\u8bd5\u7ed3\u679c<\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-9f3d908 elementor-widget elementor-widget-text-editor\" data-id=\"9f3d908\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p style=\"text-align: justify;\">\u5728\u4e0d\u540c\u8f6c\u6570(100\u3001150\u3001300\u548c800\u5faa\u73af)\u4e0b\uff0c\u5bf9\u6bcf\u4e2a\u6837\u54c1\u8fdb\u884c\u4e86\u56db\u6b21\u9488\u5bf9\u76d8\u78e8\u635f\u8bd5\u9a8c\uff0c\u4ee5\u76d1\u6d4b\u78e8\u635f\u7684\u6f14\u53d8\u3002\u5728\u8fdb\u884c\u78e8\u635f\u6d4b\u8bd5\u4e4b\u524d\uff0c\u7528NANOVEA 3D\u975e\u63a5\u89e6\u5256\u9762\u4eea\u6d4b\u91cf\u6837\u54c1\u7684\u8868\u9762\u5f62\u8c8c\uff0c\u4ee5\u91cf\u5316\u8868\u9762\u7c97\u7cd9\u5ea6\u3002\u6240\u6709\u6837\u54c1\u7684\u8868\u9762\u7c97\u7cd9\u5ea6\u5747\u7ea6\u4e3a1 \u03bcm\uff0c\u5982\u56fe1\u6240\u793a\u3002COF\u5728\u78e8\u635f\u8bd5\u9a8c\u4e2d\u539f\u5730\u8bb0\u5f55\uff0c\u5982\u56fe2\u6240\u793a\u3002\u56fe4\u4e3a100\u3001150\u3001300\u548c800\u5faa\u73af\u540e\u7684\u78e8\u635f\u8f68\u8ff9\u6f14\u53d8\uff0c\u56fe3\u4e3a\u4e0d\u540c\u6837\u54c1\u5728\u78e8\u635f\u8fc7\u7a0b\u4e0d\u540c\u9636\u6bb5\u7684\u5e73\u5747\u78e8\u635f\u7387\u3002<\/p><p>\u00a0<\/p><p style=\"text-align: justify;\">\u4e0e\u5176\u4ed6\u4e09\u79cd\u6837\u54c1\u7684COF\u503c~0.07\u76f8\u6bd4\uff0c\u6837\u54c1a\u7684COF\u503c\u5728\u5f00\u59cb\u65f6\u8981\u9ad8\u5f97\u591a\uff0c\u4e3a~0.15\uff0c\u7ecf\u8fc7300\u6b21\u78e8\u635f\u5faa\u73af\u540e\uff0cCOF\u503c\u9010\u6e10\u589e\u52a0\uff0c\u7a33\u5b9a\u5728~0.3\u3002\u5982\u6b64\u9ad8\u7684COF\u52a0\u901f\u4e86\u78e8\u635f\u8fc7\u7a0b\uff0c\u5e76\u4ea7\u751f\u4e86\u5927\u91cf\u7684\u6cb9\u6f06\u788e\u7247\uff0c\u5982\u56fe4\u6240\u793a\u2014\u2014\u6837\u54c1a\u7684\u9762\u6f06\u5728\u524d100\u8f6c\u4e2d\u5df2\u7ecf\u5f00\u59cb\u88ab\u53bb\u9664\u3002\u5982\u56fe3\u6240\u793a\uff0c\u6837\u54c1A\u5728\u524d300\u4e2a\u5faa\u73af\u4e2d\u78e8\u635f\u7387\u6700\u9ad8\uff0c\u4e3a~5 \u03bcm2\/N\uff0c\u7531\u4e8e\u91d1\u5c5e\u57fa\u4f53\u7684\u8010\u78e8\u6027\u8f83\u597d\uff0c\u78e8\u635f\u7387\u7565\u5fae\u4e0b\u964d\u5230~3.5 \u03bcm2\/N\u3002\u6837\u54c1C\u7684\u9762\u6f06\u5728150\u6b21\u78e8\u635f\u540e\u5f00\u59cb\u5931\u6548\uff0c\u5982\u56fe4\u6240\u793a\uff0c\u56fe2\u4e2dCOF\u7684\u589e\u52a0\u4e5f\u8bf4\u660e\u4e86\u8fd9\u4e00\u70b9\u3002<\/p><p>\u00a0<\/p><p style=\"text-align: justify;\">\u76f8\u6bd4\u4e4b\u4e0b\uff0c\u6837\u54c1B\u548c\u6837\u54c1D\u8868\u73b0\u51fa\u589e\u5f3a\u7684\u6469\u64e6\u5b66\u6027\u80fd\u3002\u6837\u54c1B\u5728\u6574\u4e2a\u6d4b\u8bd5\u8fc7\u7a0b\u4e2d\u4fdd\u6301\u8f83\u4f4e\u7684COF - COF\u4ece~0.05\u8f7b\u5fae\u589e\u52a0\u5230~0.1\u3002\u8fd9\u6837\u7684\u6da6\u6ed1\u6548\u679c\u5927\u5927\u63d0\u9ad8\u4e86\u5b83\u7684\u8010\u78e8\u6027-\u9762\u6f06\u5728800\u6b21\u78e8\u635f\u5faa\u73af\u540e\u4ecd\u7136\u5bf9\u5e95\u6f06\u63d0\u4f9b\u4f18\u8d8a\u7684\u4fdd\u62a4\u3002\u6837\u54c1B\u5728800\u6b21\u5faa\u73af\u65f6\u7684\u6700\u4f4e\u5e73\u5747\u78e8\u635f\u7387\u4ec5\u4e3a~0.77 \u03bcm2\/N\u3002\u6837\u54c1D\u7684\u9762\u6f06\u5728375\u6b21\u5faa\u73af\u540e\u5f00\u59cb\u5206\u5c42\uff0c\u4ece\u56fe2\u4e2dCOF\u7684\u7a81\u7136\u589e\u52a0\u53ef\u4ee5\u770b\u51fa\u3002\u6837\u54c1D\u5728800\u6b21\u5faa\u73af\u65f6\u7684\u5e73\u5747\u78e8\u635f\u7387\u7ea6\u4e3a1.1 \u03bcm2\/N\u3002<\/p><p>\u00a0<\/p><p style=\"text-align: justify;\">\u4e0e\u4f20\u7edf\u7684Taber\u78e8\u635f\u6d4b\u91cf\u76f8\u6bd4\uff0cNANOVEA\u6469\u64e6\u4eea\u63d0\u4f9b\u4e86\u826f\u597d\u63a7\u5236\u7684\u53ef\u91cf\u5316\u548c\u53ef\u9760\u7684\u78e8\u635f\u8bc4\u4f30\uff0c\u786e\u4fdd\u4e86\u5546\u4e1a\u5730\u677f\/\u6c7d\u8f66\u6d82\u6599\u7684\u53ef\u91cd\u590d\u6027\u8bc4\u4f30\u548c\u8d28\u91cf\u63a7\u5236\u3002\u6b64\u5916\uff0c\u539f\u4f4dCOF\u6d4b\u91cf\u7684\u80fd\u529b\u4f7f\u7528\u6237\u80fd\u591f\u5c06\u78e8\u635f\u8fc7\u7a0b\u7684\u4e0d\u540c\u9636\u6bb5\u4e0eCOF\u7684\u6f14\u53d8\u8054\u7cfb\u8d77\u6765\uff0c\u8fd9\u5bf9\u4e8e\u63d0\u9ad8\u5bf9\u5404\u79cd\u6cb9\u6f06\u6d82\u5c42\u7684\u78e8\u635f\u673a\u5236\u548c\u6469\u64e6\u5b66\u7279\u6027\u7684\u57fa\u672c\u8ba4\u8bc6\u81f3\u5173\u91cd\u8981\u3002<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-7311885 elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"7311885\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-b11fd5d\" data-id=\"b11fd5d\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<section class=\"elementor-section elementor-inner-section elementor-element elementor-element-f59c5b1 elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"f59c5b1\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-inner-column elementor-element elementor-element-7a5dc99\" data-id=\"7a5dc99\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-40fab7c elementor-widget elementor-widget-image\" data-id=\"40fab7c\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img loading=\"lazy\" decoding=\"async\" width=\"366\" height=\"345\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2022\/05\/Industrial-Coatings-Profilometry.jpg\" class=\"attachment-large size-large wp-image-20026\" alt=\"\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-inner-column elementor-element elementor-element-24174e9\" data-id=\"24174e9\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-964c701 elementor-widget elementor-widget-image\" data-id=\"964c701\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img loading=\"lazy\" decoding=\"async\" width=\"366\" height=\"345\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2022\/05\/Industrial-Coatings-Roughness.jpg\" class=\"attachment-large size-large wp-image-20027\" alt=\"\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-inner-section elementor-element elementor-element-feddc4b elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"feddc4b\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-inner-column elementor-element elementor-element-3bed450\" data-id=\"3bed450\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-58312f2 elementor-widget elementor-widget-image\" data-id=\"58312f2\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img loading=\"lazy\" decoding=\"async\" width=\"366\" height=\"345\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2022\/05\/Industrial-Paint-Roughness.jpg\" class=\"attachment-large size-large wp-image-20031\" alt=\"\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-inner-column elementor-element elementor-element-2a63829\" data-id=\"2a63829\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-641c302 elementor-widget elementor-widget-image\" data-id=\"641c302\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img loading=\"lazy\" decoding=\"async\" width=\"366\" height=\"345\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2022\/05\/Industrial-Paint-Testing.jpg\" class=\"attachment-large size-large wp-image-20035\" alt=\"\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<div class=\"elementor-element elementor-element-4103861 elementor-widget elementor-widget-text-editor\" data-id=\"4103861\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p style=\"text-align: center;\"><span class=\"fontstyle0\" style=\"color: #1b96cf;\">\u56fe1: <\/span><span class=\"fontstyle0\" style=\"color: #1b96cf;\"><span style=\"color: #000000;\"><span class=\"fontstyle0\">\u6d82\u6599\u6837\u54c1\u7684\u4e09\u7ef4\u5f62\u6001\u548c\u7c97\u7cd9\u5ea6\u3002<\/span>\n<\/span><\/span><\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<section class=\"elementor-section elementor-inner-section elementor-element elementor-element-eea6b5a elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"eea6b5a\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-inner-column elementor-element elementor-element-7e36f39\" data-id=\"7e36f39\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-868b4e2 elementor-widget elementor-widget-image\" data-id=\"868b4e2\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img loading=\"lazy\" decoding=\"async\" width=\"719\" height=\"508\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2022\/05\/Industrial-Coatings-COF.jpg\" class=\"attachment-large size-large wp-image-20024\" alt=\"\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-0cfdbaa elementor-widget elementor-widget-text-editor\" data-id=\"0cfdbaa\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p style=\"text-align: center;\"><span class=\"fontstyle0\" style=\"color: #1b96cf;\">\u56fe2: <\/span><span style=\"color: #000000;\"><span class=\"fontstyle0\">\u5728\u5f15\u811a\u78c1\u76d8\u6d4b\u8bd5\u671f\u95f4\uff0cCOF\u3002<\/span><\/span><\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-inner-column elementor-element elementor-element-5864534\" data-id=\"5864534\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-9ee2592 elementor-widget elementor-widget-image\" data-id=\"9ee2592\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img loading=\"lazy\" decoding=\"async\" width=\"719\" height=\"508\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2022\/05\/Industrial-Coating-Wear-Test.jpg\" class=\"attachment-large size-large wp-image-20023\" alt=\"\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-6f42a0a elementor-widget elementor-widget-text-editor\" data-id=\"6f42a0a\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p style=\"text-align: center;\"><span class=\"fontstyle0\" style=\"color: #1b96cf;\">\u56fe3: <\/span><span style=\"color: #000000;\"><span class=\"fontstyle0\">\u4e0d\u540c\u6d82\u6599\u7684\u78e8\u635f\u7387\u7684\u6f14\u53d8\u3002<\/span><\/span><\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<div class=\"elementor-element elementor-element-4015260 elementor-widget elementor-widget-image\" data-id=\"4015260\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img loading=\"lazy\" decoding=\"async\" width=\"1024\" height=\"801\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2022\/05\/Industrial-Paint-Wear-Test.jpg\" class=\"attachment-large size-large wp-image-20037\" alt=\"\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-56e7fda elementor-widget elementor-widget-text-editor\" data-id=\"56e7fda\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p style=\"text-align: center;\"><span class=\"fontstyle0\" style=\"color: #1b96cf;\">\u56fe4: <\/span><span class=\"fontstyle0\" style=\"color: #1b96cf;\"><span style=\"color: #000000;\"><span class=\"fontstyle0\">\u9489\u76d8\u8bd5\u9a8c\u671f\u95f4\u78e8\u635f\u75d5\u8ff9\u7684\u6f14\u53d8\u3002<\/span>\n<\/span><\/span><\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-ec03633 elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"ec03633\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-no\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-c910bc7\" data-id=\"c910bc7\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-99fcb17 elementor-widget elementor-widget-heading\" data-id=\"99fcb17\" data-element_type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\">\u5212\u75d5\u6d4b\u8bd5\u7ed3\u679c<\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-4398642 elementor-widget elementor-widget-text-editor\" data-id=\"4398642\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p style=\"text-align: justify;\">\u56fe5\u663e\u793a\u4e86\u4ee5\u6837\u54c1A\u4e3a\u4f8b\uff0c\u6cd5\u5411\u529b\u3001\u6469\u64e6\u529b\u548c\u771f\u5b9e\u6df1\u5ea6\u4e0e\u5212\u75d5\u957f\u5ea6\u7684\u5173\u7cfb\u56fe\u3002\u53ef\u4ee5\u5b89\u88c5\u4e00\u4e2a\u53ef\u9009\u7684\u58f0\u53d1\u5c04\u6a21\u5757\u6765\u63d0\u4f9b\u66f4\u591a\u4fe1\u606f\u3002\u968f\u7740\u6cd5\u5411\u8f7d\u8377\u7684\u7ebf\u6027\u589e\u52a0\uff0c\u538b\u75d5\u5c16\u7aef\u9010\u6e10\u4e0b\u6c89\u5230\u88ab\u6d4b\u6837\u54c1\u4e2d\uff0c\u8fd9\u53cd\u6620\u5728\u771f\u5b9e\u6df1\u5ea6\u7684\u9010\u6e10\u589e\u52a0\u4e0a\u3002\u6469\u64e6\u529b\u548c\u771f\u5b9e\u6df1\u5ea6\u66f2\u7ebf\u7684\u659c\u7387\u53d8\u5316\u53ef\u4ee5\u4f5c\u4e3a\u6d82\u5c42\u5f00\u59cb\u51fa\u73b0\u6545\u969c\u7684\u542b\u4e49\u4e4b\u4e00\u3002<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-fe155f9 elementor-widget elementor-widget-image\" data-id=\"fe155f9\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img loading=\"lazy\" decoding=\"async\" width=\"926\" height=\"495\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2022\/05\/Industrial-Coating-Scratch-Test.jpg\" class=\"attachment-large size-large wp-image-20044\" alt=\"\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-43838d4 elementor-widget elementor-widget-text-editor\" data-id=\"43838d4\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p style=\"text-align: center;\"><span class=\"fontstyle0\" style=\"color: #1b96cf;\">\u56fe5: <\/span><span class=\"fontstyle0\" style=\"color: #1b96cf;\"><span style=\"color: #000000;\"><span class=\"fontstyle0\">\u6cd5\u5411\u529b\u3001\u6469\u64e6\u529b\u548c\u771f\u5b9e\u6df1\u5ea6\u4e0e\u5212\u75d5\u957f\u5ea6\u7684\u5173\u7cfb\u3002\n\u6700\u5927\u8f7d\u8377\u4e3a5N\u7684\u6837\u54c1A\u7684\u5212\u75d5\u6d4b\u8bd5\u3002<\/span>\n<\/span><\/span><\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-4762328 elementor-widget elementor-widget-text-editor\" data-id=\"4762328\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p style=\"text-align: justify;\">\u56fe6\u548c\u56fe7\u663e\u793a\u4e86\u5728\u6700\u5927\u8f7d\u8377\u4e3a5N\u548c35N\u7684\u60c5\u51b5\u4e0b\u6d4b\u8bd5\u7684\u6240\u6709\u56db\u4e2a\u6cb9\u6f06\u6837\u54c1\u7684\u5168\u90e8\u5212\u75d5\u3002\u6837\u54c1D\u9700\u8981\u66f4\u9ad8\u7684\u8d1f\u8377\uff0c\u537350N\u624d\u80fd\u4f7f\u5e95\u6f06\u8131\u5c42\u3002\u57285N\u7684\u6700\u7ec8\u8f7d\u8377\u4e0b\u7684\u5212\u75d5\u6d4b\u8bd5\uff08\u56fe6\uff09\u8bc4\u4f30\u4e86\u9762\u6f06\u7684\u5185\u805a\/\u7c98\u9644\u5931\u6548\uff0c\u800c\u572835N\u7684\u6d4b\u8bd5\uff08\u56fe7\uff09\u8bc4\u4f30\u4e86\u5e95\u6f06\u7684\u5206\u5c42\u3002\u663e\u5fae\u7167\u7247\u4e2d\u7684\u7bad\u5934\u8868\u793a\u9876\u5c42\u6d82\u6599\u6216\u5e95\u5c42\u6d82\u6599\u5f00\u59cb\u4ece\u5e95\u5c42\u6216\u57fa\u6750\u4e0a\u5b8c\u5168\u8131\u843d\u7684\u70b9\u3002\u5728\u8fd9\u4e00\u70b9\u4e0a\u7684\u8f7d\u8377\uff0c\u5373\u6240\u8c13\u7684\u4e34\u754c\u8f7d\u8377\uff0cLc\uff0c\u662f\u7528\u6765\u6bd4\u8f83\u6d82\u6599\u7684\u5185\u805a\u529b\u6216\u7c98\u5408\u529b\u7684\uff0c\u5982\u88681\u6240\u603b\u7ed3\u7684\u3002<\/p><p style=\"text-align: justify;\">\u00a0<\/p><p style=\"text-align: justify;\">\u5f88\u660e\u663e\uff0c\u6cb9\u6f06\u6837\u54c1D\u5177\u6709\u6700\u597d\u7684\u754c\u9762\u9644\u7740\u529b\u2014\u2014\u5728\u6cb9\u6f06\u5206\u5c42\u5904\u663e\u793a\u51fa\u6700\u9ad8\u7684Lc\u503c4.04 N\uff0c\u5728\u5e95\u6f06\u5206\u5c42\u5904\u663e\u793a\u51fa36.61 N\u3002\u6837\u54c1B\u663e\u793a\u51fa\u7b2c\u4e8c\u597d\u7684\u8010\u522e\u6027\u3002\u4ece\u5212\u75d5\u5206\u6790\u4e2d\uff0c\u6211\u4eec\u53d1\u73b0\u6d82\u6599\u914d\u65b9\u7684\u4f18\u5316\u5bf9\u4e19\u70ef\u9178\u5730\u677f\u6d82\u6599\u7684\u529b\u5b66\u6027\u80fd\uff0c\u6216\u66f4\u5177\u4f53\u5730\u8bf4\uff0c\u8010\u5212\u75d5\u6027\u548c\u7c98\u9644\u6027\u81f3\u5173\u91cd\u8981\u3002<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-214f524 elementor-widget elementor-widget-image\" data-id=\"214f524\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img loading=\"lazy\" decoding=\"async\" width=\"1024\" height=\"225\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2022\/05\/Industrial-Paint-QC.jpg\" class=\"attachment-large size-large wp-image-20030\" alt=\"\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-a992b7a elementor-widget elementor-widget-text-editor\" data-id=\"a992b7a\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p style=\"text-align: center;\"><span class=\"fontstyle0\" style=\"color: #1b96cf;\">\u88681: <\/span><span class=\"fontstyle0\" style=\"color: #1b96cf;\"><span style=\"color: #000000;\"><span class=\"fontstyle0\">\u5173\u952e\u8d1f\u8377\u7684\u603b\u7ed3\u3002<\/span>\n<\/span><\/span><\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-39ae57e elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"39ae57e\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-20028cc\" data-id=\"20028cc\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-762a9a3 elementor-widget elementor-widget-image\" data-id=\"762a9a3\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img loading=\"lazy\" decoding=\"async\" width=\"1024\" height=\"196\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2022\/05\/Industrial-Coating-Scratch.jpg\" class=\"attachment-large size-large wp-image-20042\" alt=\"\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-6e5aa76 elementor-widget elementor-widget-image\" data-id=\"6e5aa76\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img loading=\"lazy\" decoding=\"async\" width=\"1024\" height=\"198\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2022\/05\/Industrial-Coating-Scratch-Testing.jpg\" class=\"attachment-large size-large wp-image-20041\" alt=\"\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-e9a0a91 elementor-widget elementor-widget-image\" data-id=\"e9a0a91\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img loading=\"lazy\" decoding=\"async\" width=\"1024\" height=\"198\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2022\/05\/Industrial-Coating-Scratch-Tester.jpg\" class=\"attachment-large size-large wp-image-20040\" alt=\"\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-ef0ba5a elementor-widget elementor-widget-image\" data-id=\"ef0ba5a\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img loading=\"lazy\" decoding=\"async\" width=\"1024\" height=\"198\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2022\/05\/Industrial-Coating-Scratch-QC-Test.jpg\" class=\"attachment-large size-large wp-image-20039\" alt=\"\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-b136a8f elementor-widget elementor-widget-text-editor\" data-id=\"b136a8f\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p style=\"text-align: center;\"><span class=\"fontstyle0\" style=\"color: #1b96cf;\">\u56fe6: <\/span><span class=\"fontstyle0\" style=\"color: #1b96cf;\"><span style=\"color: #000000;\"><span class=\"fontstyle0\">\u6700\u5927\u8d1f\u8377\u4e3a5N\u7684\u5b8c\u5168\u5212\u75d5\u7684\u663e\u5fae\u7167\u7247\u3002<\/span>\n<\/span><\/span><\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-3dd028d elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"3dd028d\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-36cb163\" data-id=\"36cb163\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-d35b065 elementor-widget elementor-widget-image\" data-id=\"d35b065\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img loading=\"lazy\" decoding=\"async\" width=\"1024\" height=\"198\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2022\/05\/Industrial-Paint-Scratch-Test.jpg\" class=\"attachment-large size-large wp-image-20033\" alt=\"\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-daf897a elementor-widget elementor-widget-image\" data-id=\"daf897a\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img loading=\"lazy\" decoding=\"async\" width=\"1024\" height=\"198\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2022\/05\/Industrial-Paint-Scratch-Testing.jpg\" class=\"attachment-large size-large wp-image-20034\" alt=\"\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-20c9e99 elementor-widget elementor-widget-image\" data-id=\"20c9e99\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img loading=\"lazy\" decoding=\"async\" width=\"1024\" height=\"198\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2022\/05\/Industrial-Paint-Lab-Testing.jpg\" class=\"attachment-large size-large wp-image-20029\" alt=\"\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-f7b4a00 elementor-widget elementor-widget-image\" data-id=\"f7b4a00\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img loading=\"lazy\" decoding=\"async\" width=\"1024\" height=\"148\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2022\/05\/Industrial-Paint-Scratch-QC-Test.jpg\" class=\"attachment-large size-large wp-image-20032\" alt=\"\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-9a86977 elementor-widget elementor-widget-text-editor\" data-id=\"9a86977\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p style=\"text-align: center;\"><span class=\"fontstyle0\" style=\"color: #1b96cf;\">\u56fe7: <\/span><span class=\"fontstyle0\" style=\"color: #1b96cf;\"><span style=\"color: #000000;\"><span class=\"fontstyle0\">\u6700\u5927\u8d1f\u8377\u4e3a35N\u7684\u5b8c\u5168\u5212\u75d5\u7684\u663e\u5fae\u7167\u7247\u3002<\/span>\n<\/span><\/span><\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-c8c9bdf elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"c8c9bdf\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-724e51f\" data-id=\"724e51f\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-ec6977f elementor-widget elementor-widget-heading\" data-id=\"ec6977f\" data-element_type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\">\u7ed3\u8bba<\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-dcde8ed elementor-widget elementor-widget-text-editor\" data-id=\"dcde8ed\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p style=\"text-align: justify;\">\u4e0e\u4f20\u7edf\u7684Taber\u78e8\u8680\u6d4b\u91cf\u76f8\u6bd4\uff0cNANOVEA\u673a\u68b0\u6d4b\u8bd5\u4eea\u548c\u6469\u64e6\u4eea\u662f\u5546\u4e1a\u5730\u677f\u548c\u6c7d\u8f66\u6d82\u6599\u8bc4\u4f30\u548c\u8d28\u91cf\u63a7\u5236\u7684\u5353\u8d8a\u5de5\u5177\u3002NANOVEA\u673a\u68b0\u6d4b\u8bd5\u4eea\u5728\u5212\u75d5\u6a21\u5f0f\u4e0b\u53ef\u4ee5\u68c0\u6d4b\u6d82\u5c42\u7cfb\u7edf\u4e2d\u7684\u9644\u7740\u529b\/\u5185\u805a\u529b\u95ee\u9898\u3002NANOVEA\u6469\u64e6\u4eea\u5bf9\u6d82\u6599\u7684\u8010\u78e8\u6027\u548c\u6469\u64e6\u7cfb\u6570\u63d0\u4f9b\u4e86\u826f\u597d\u63a7\u5236\u7684\u53ef\u91cf\u5316\u548c\u53ef\u91cd\u590d\u7684\u6469\u64e6\u5b66\u5206\u6790\u3002<\/p><p>\u00a0<\/p><p>\u57fa\u4e8e\u5bf9\u672c\u7814\u7a76\u4e2d\u6d4b\u8bd5\u7684\u6c34\u57fa\u4e19\u70ef\u9178\u5730\u677f\u6d82\u6599\u7684\u7efc\u5408\u6469\u64e6\u5b66\u548c\u673a\u68b0\u5206\u6790\uff0c\u6211\u4eec\u8868\u660e\u6837\u54c1B\u62e5\u6709\u6700\u4f4e\u7684COF\u548c\u78e8\u635f\u7387\uff0c\u4ee5\u53ca\u7b2c\u4e8c\u597d\u7684\u8010\u522e\u64e6\u6027\uff0c\u800c\u6837\u54c1D\u8868\u73b0\u51fa\u6700\u597d\u7684\u8010\u522e\u64e6\u6027\u548c\u7b2c\u4e8c\u597d\u7684\u8010\u78e8\u6027\u3002\u8fd9\u4e00\u8bc4\u4f30\u4f7f\u6211\u4eec\u80fd\u591f\u8bc4\u4f30\u548c\u9009\u62e9\u9488\u5bf9\u4e0d\u540c\u5e94\u7528\u73af\u5883\u9700\u6c42\u7684\u6700\u4f73\u5019\u9009\u4eba\u3002<\/p><p>\u00a0<\/p><p>NANOVEA\u673a\u68b0\u6d4b\u8bd5\u4eea\u7684\u7eb3\u7c73\u548c\u5fae\u6a21\u5757\u90fd\u5305\u62ecISO\u548cASTM\u517c\u5bb9\u7684\u538b\u75d5\uff0c\u5212\u75d5\u548c\u78e8\u635f\u6d4b\u8bd5\u6a21\u5f0f\uff0c\u63d0\u4f9b\u4e86\u6700\u5e7f\u6cdb\u7684\u6d4b\u8bd5\u8303\u56f4\uff0c\u53ef\u5728\u5355\u4e2a\u6a21\u5757\u4e0a\u8fdb\u884c\u6cb9\u6f06\u8bc4\u4f30\u3002NANOVEA\u6469\u64e6\u8ba1\u4f7f\u7528\u7b26\u5408ISO\u548cASTM\u6807\u51c6\u7684\u65cb\u8f6c\u548c\u7ebf\u6027\u6a21\u5f0f\u63d0\u4f9b\u7cbe\u786e\u548c\u53ef\u91cd\u590d\u7684\u78e8\u635f\u548c\u6469\u64e6\u6d4b\u8bd5\uff0c\u5e76\u53ef\u5728\u4e00\u4e2a\u9884\u5148\u96c6\u6210\u7684\u7cfb\u7edf\u4e2d\u63d0\u4f9b\u53ef\u9009\u7684\u9ad8\u6e29\u78e8\u635f\u3001\u6da6\u6ed1\u548c\u6469\u64e6\u8150\u8680\u6a21\u5757\u3002NANOVEA\u65e0\u4e0e\u4f26\u6bd4\u7684\u8303\u56f4\u662f\u786e\u5b9a\u8584\u6216\u539a\u3001\u8f6f\u6216\u786c\u6d82\u5c42\u3001\u8584\u819c\u548c\u57fa\u6750\u7684\u5168\u5957\u673a\u68b0\/\u6469\u64e6\u5b66\u6027\u80fd\u7684\u7406\u60f3\u89e3\u51b3\u65b9\u6848\uff0c\u5305\u62ec\u786c\u5ea6\u3001\u6768\u6c0f\u6a21\u91cf\u3001\u65ad\u88c2\u97e7\u6027\u3001\u9644\u7740\u529b\u3001\u8010\u78e8\u6027\u548c\u8bb8\u591a\u5176\u4ed6\u6027\u80fd\u3002\u53ef\u9009NANOVEA\u975e\u63a5\u89e6\u5f0f\u5149\u5b66\u5256\u9762\u4eea\u53ef\u7528\u4e8e\u5212\u75d5\u548c\u78e8\u635f\u8f68\u8ff9\u7684\u9ad8\u5206\u8fa8\u7387\u4e09\u7ef4\u6210\u50cf\uff0c\u4ee5\u53ca\u5176\u4ed6\u8868\u9762\u6d4b\u91cf\uff0c\u5982\u7c97\u7cd9\u5ea6\u3002<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-e71b01c elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"e71b01c\" data-element_type=\"section\" data-settings=\"{&quot;background_background&quot;:&quot;classic&quot;}\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-4393a2f\" data-id=\"4393a2f\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-53db75e elementor-widget elementor-widget-heading\" data-id=\"53db75e\" data-element_type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\"><b>\u73b0\u5728\uff0c\u8ba9\u6211\u4eec\u6765\u8c08\u8c08\u4f60\u7684\u7533\u8bf7<\/b><\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-d73f295 live-chat elementor-align-center elementor-widget elementor-widget-button\" data-id=\"d73f295\" data-element_type=\"widget\" data-widget_type=\"button.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<div class=\"elementor-button-wrapper\">\n\t\t\t\t\t<a class=\"elementor-button elementor-button-link elementor-size-md\" href=\"https:\/\/nanovea.com\/contact\/live-chat\/\" id=\"live-chat\">\n\t\t\t\t\t\t<span class=\"elementor-button-content-wrapper\">\n\t\t\t\t\t\t\t\t\t<span class=\"elementor-button-text\">\u5b9e\u65f6\u804a\u5929<\/span>\n\t\t\t\t\t<\/span>\n\t\t\t\t\t<\/a>\n\t\t\t\t<\/div>\n\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<\/div>","protected":false},"excerpt":{"rendered":"<p>INDUSTRIAL COATING SCRATCH AND WEAR EVALUATION USING A TRIBOMETER Prepared by DUANJIE LI, PhD &amp; ANDREA HERRMANN INTRODUCTION Acrylic urethane paint is a type of fast-dry protective coating widely used in a variety of industrial applications, such as floor paint, auto paint, and others. When used as floor paint, it can serve areas with heavy [&hellip;]<\/p>\n","protected":false},"author":1,"featured_media":21169,"comment_status":"open","ping_status":"open","sticky":false,"template":"","format":"standard","meta":{"_exactmetrics_skip_tracking":false,"_exactmetrics_sitenote_active":false,"_exactmetrics_sitenote_note":"","_exactmetrics_sitenote_category":0,"footnotes":""},"categories":[7,348,349,337,351,335,373,345,346,336],"tags":[],"class_list":["post-20021","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-application-notes","category-friction-testing-coefficient-of-friction","category-laboratory-testing","category-mechanical-testing","category-profilometry-roughness-finish","category-profilometry-testing","category-rotational-tribology","category-scratch-testing-adhesive-failure","category-scratch-testing-cohesive-failure","category-tribology-testing"],"_links":{"self":[{"href":"https:\/\/nanovea.com\/zh\/wp-json\/wp\/v2\/posts\/20021","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/nanovea.com\/zh\/wp-json\/wp\/v2\/posts"}],"about":[{"href":"https:\/\/nanovea.com\/zh\/wp-json\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"https:\/\/nanovea.com\/zh\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/nanovea.com\/zh\/wp-json\/wp\/v2\/comments?post=20021"}],"version-history":[{"count":42,"href":"https:\/\/nanovea.com\/zh\/wp-json\/wp\/v2\/posts\/20021\/revisions"}],"predecessor-version":[{"id":23862,"href":"https:\/\/nanovea.com\/zh\/wp-json\/wp\/v2\/posts\/20021\/revisions\/23862"}],"wp:featuredmedia":[{"embeddable":true,"href":"https:\/\/nanovea.com\/zh\/wp-json\/wp\/v2\/media\/21169"}],"wp:attachment":[{"href":"https:\/\/nanovea.com\/zh\/wp-json\/wp\/v2\/media?parent=20021"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"https:\/\/nanovea.com\/zh\/wp-json\/wp\/v2\/categories?post=20021"},{"taxonomy":"post_tag","embeddable":true,"href":"https:\/\/nanovea.com\/zh\/wp-json\/wp\/v2\/tags?post=20021"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}