{"id":22017,"date":"2023-05-01T18:42:24","date_gmt":"2023-05-01T18:42:24","guid":{"rendered":"https:\/\/nanovea.com\/?p=22017"},"modified":"2025-05-22T19:12:25","modified_gmt":"2025-05-22T19:12:25","slug":"inspeccao-da-rugosidade-do-mapeamento-utilizando-a-profilometria-3d","status":"publish","type":"post","link":"https:\/\/nanovea.com\/pt\/roughness-mapping-inspection-using-3d-profilometry\/","title":{"rendered":"Inspe\u00e7\u00e3o de mapeamento de rugosidade usando perfilometria 3D"},"content":{"rendered":"<div data-elementor-type=\"wp-post\" data-elementor-id=\"22017\" class=\"elementor elementor-22017\" data-elementor-post-type=\"post\">\n\t\t\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-7ec3d48 elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"7ec3d48\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-c477953\" data-id=\"c477953\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-cec2c6e elementor-widget elementor-widget-heading\" data-id=\"cec2c6e\" data-element_type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h1 class=\"elementor-heading-title elementor-size-default\">INSPE\u00c7\u00c3O DE MAPEAMENTO DE RUGOSIDADE<\/h1>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-d107f9b elementor-widget elementor-widget-heading\" data-id=\"d107f9b\" data-element_type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\">USANDO A PROFILOMETRIA 3D<\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-73c118d elementor-widget elementor-widget-image\" data-id=\"73c118d\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img fetchpriority=\"high\" decoding=\"async\" width=\"768\" height=\"224\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2023\/05\/Roughness-Mapping-Profilometer-NANOVEA.jpg\" class=\"attachment-medium_large size-medium_large wp-image-22022\" alt=\"\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-97cc106 elementor-widget elementor-widget-heading\" data-id=\"97cc106\" data-element_type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\">Preparado por<\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-95aa94e elementor-widget elementor-widget-heading\" data-id=\"95aa94e\" data-element_type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\">DUANJIE, PhD<\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-c14383d elementor-widget elementor-widget-spacer\" data-id=\"c14383d\" data-element_type=\"widget\" data-widget_type=\"spacer.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t<div class=\"elementor-spacer\">\n\t\t\t<div class=\"elementor-spacer-inner\"><\/div>\n\t\t<\/div>\n\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-753c1f3 elementor-section-height-min-height elementor-section-content-middle elementor-reverse-mobile elementor-section-boxed elementor-section-height-default elementor-section-items-middle\" data-id=\"753c1f3\" data-element_type=\"section\" data-settings=\"{&quot;background_background&quot;:&quot;classic&quot;}\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-top-column elementor-element elementor-element-f2074e4 elementor-hidden-phone\" data-id=\"f2074e4\" data-element_type=\"column\" data-settings=\"{&quot;background_background&quot;:&quot;classic&quot;}\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-c0f91f8 elementor-widget elementor-widget-spacer\" data-id=\"c0f91f8\" data-element_type=\"widget\" data-widget_type=\"spacer.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t<div class=\"elementor-spacer\">\n\t\t\t<div class=\"elementor-spacer-inner\"><\/div>\n\t\t<\/div>\n\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-top-column elementor-element elementor-element-b259d86\" data-id=\"b259d86\" data-element_type=\"column\" data-settings=\"{&quot;background_background&quot;:&quot;classic&quot;}\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-62f2a44 elementor-widget elementor-widget-heading\" data-id=\"62f2a44\" data-element_type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\">INTRODU\u00c7\u00c3O<\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-9ab0009 elementor-widget elementor-widget-text-editor\" data-id=\"9ab0009\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p>A rugosidade e a textura da superf\u00edcie s\u00e3o fatores cr\u00edticos que afetam a qualidade final e o desempenho de um produto. Uma compreens\u00e3o completa da rugosidade, da textura e da consist\u00eancia da superf\u00edcie \u00e9 essencial para selecionar as melhores medidas de processamento e controle. A inspe\u00e7\u00e3o em linha r\u00e1pida, quantific\u00e1vel e confi\u00e1vel das superf\u00edcies dos produtos \u00e9 necess\u00e1ria para identificar os produtos defeituosos a tempo e otimizar as condi\u00e7\u00f5es da linha de produ\u00e7\u00e3o.<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-d440447 elementor-widget elementor-widget-heading\" data-id=\"d440447\" data-element_type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\">IMPORT\u00c2NCIA DO PROFIL\u00d4METRO 3D SEM CONTATO PARA A INSPE\u00c7\u00c3O DE SUPERF\u00cdCIE EM LINHA<\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-966ab4d elementor-widget elementor-widget-text-editor\" data-id=\"966ab4d\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p>Defeitos superficiais em produtos resultam do processamento de materiais e da fabrica\u00e7\u00e3o do produto. A inspe\u00e7\u00e3o de qualidade de superf\u00edcie em linha garante o mais rigoroso controle de qualidade dos produtos finais. NANOVEA <a href=\"https:\/\/nanovea.com\/profilometers\/\">Perfiladores \u00f3pticos 3D sem contato<\/a> utilizam a tecnologia Chromatic Light com capacidade exclusiva para determinar a rugosidade de uma amostra sem contato. O sensor de linha permite a digitaliza\u00e7\u00e3o do perfil 3D de uma grande superf\u00edcie em alta velocidade. O limite de rugosidade, calculado em tempo real pelo software de an\u00e1lise, serve como uma ferramenta de aprova\u00e7\u00e3o\/reprova\u00e7\u00e3o r\u00e1pida e confi\u00e1vel.<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-1ac4bd1 elementor-reverse-mobile elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"1ac4bd1\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-2deb3a7\" data-id=\"2deb3a7\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<section class=\"elementor-section elementor-inner-section elementor-element elementor-element-71e5e88 elementor-reverse-mobile elementor-section-full_width elementor-reverse-tablet elementor-section-height-default elementor-section-height-default\" data-id=\"71e5e88\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-no\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-inner-column elementor-element elementor-element-6e1b946\" data-id=\"6e1b946\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-031e9e3 elementor-widget elementor-widget-text-editor\" data-id=\"031e9e3\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p style=\"text-align: left;\">OBJETIVO DA MEDI\u00c7\u00c3O<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-cba91d4 elementor-widget elementor-widget-text-editor\" data-id=\"cba91d4\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p><em>Neste estudo, o NANOVEA ST400 equipado com um sensor de alta velocidade \u00e9 usado para inspecionar a superf\u00edcie de uma amostra de teflon com defeito para mostrar a capacidade do NANOVEA<\/em><\/p><p><em>Pro\ufb01l\u00f4metros sem contato para fornecer inspe\u00e7\u00e3o de superf\u00edcie r\u00e1pida e confi\u00e1vel em uma linha de produ\u00e7\u00e3o.<\/em><\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-71bd4f7 elementor-widget elementor-widget-text-editor\" data-id=\"71bd4f7\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p style=\"text-align: left;\">NANOVEA<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-03a2e57 elementor-widget elementor-widget-text-editor\" data-id=\"03a2e57\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p style=\"text-align: left;\">ST400<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-73dc4e0 elementor-align-left learn-more-about-instrument elementor-widget elementor-widget-button\" data-id=\"73dc4e0\" data-element_type=\"widget\" data-widget_type=\"button.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<div class=\"elementor-button-wrapper\">\n\t\t\t\t\t<a class=\"elementor-button elementor-button-link elementor-size-xs\" href=\"https:\/\/nanovea.com\/instruments\/st400\" id=\"learn-more-about-instrument\">\n\t\t\t\t\t\t<span class=\"elementor-button-content-wrapper\">\n\t\t\t\t\t\t\t\t\t<span class=\"elementor-button-text\">SAIBA MAIS<\/span>\n\t\t\t\t\t<\/span>\n\t\t\t\t\t<\/a>\n\t\t\t\t<\/div>\n\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-inner-column elementor-element elementor-element-f8bd391\" data-id=\"f8bd391\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-657905d elementor-widget elementor-widget-image\" data-id=\"657905d\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<a href=\"https:\/\/nanovea.com\/instruments\/st400\">\n\t\t\t\t\t\t\t<img decoding=\"async\" width=\"768\" height=\"776\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2020\/12\/Nanovea-Optical-Profilometry-ST400.png\" class=\"elementor-animation-grow attachment-medium_large size-medium_large wp-image-9556\" alt=\"\" \/>\t\t\t\t\t\t\t\t<\/a>\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-94e8004 elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"94e8004\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-no\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-cf2d779\" data-id=\"cf2d779\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-b24853d elementor-widget elementor-widget-heading\" data-id=\"b24853d\" data-element_type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\">RESULTADOS &amp; DISCUSS\u00c3O<\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-26b3672 elementor-widget elementor-widget-text-editor\" data-id=\"26b3672\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p style=\"text-align: left;\"><strong><em>An\u00e1lise de superf\u00edcie 3D do\u00a0<\/em><\/strong><strong style=\"color: var( --e-global-color-primary );\"><em>Amostra padr\u00e3o de rugosidade<\/em><\/strong><\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-1e5424c elementor-widget elementor-widget-text-editor\" data-id=\"1e5424c\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p style=\"text-align: left;\">A superf\u00edcie de um padr\u00e3o de rugosidade foi escaneada usando um NANOVEA ST400 equipado com um sensor de alta velocidade que gera uma linha brilhante de 192 pontos, conforme mostrado na FIGURA 1. Esses 192 pontos escaneiam a superf\u00edcie da amostra ao mesmo tempo, o que resulta em um aumento significativo da velocidade de escaneamento.<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<section class=\"elementor-section elementor-inner-section elementor-element elementor-element-ae07996 elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"ae07996\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-no\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-inner-column elementor-element elementor-element-c92af22\" data-id=\"c92af22\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-b75455c elementor-widget elementor-widget-text-editor\" data-id=\"b75455c\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p style=\"text-align: left;\">A FIGURA 2 mostra visualiza\u00e7\u00f5es em falsa cor do Mapa de Altura da Superf\u00edcie e do Mapa de Distribui\u00e7\u00e3o de Rugosidade da Amostra Padr\u00e3o de Rugosidade. Na FIGURA 2a, o padr\u00e3o de rugosidade exibe uma superf\u00edcie ligeiramente inclinada, conforme representado pelo gradiente de cores variadas em cada um dos blocos de rugosidade padr\u00e3o. Na FIGURA 2b, a distribui\u00e7\u00e3o homog\u00eanea da rugosidade \u00e9 mostrada em diferentes blocos de rugosidade, cuja cor representa a rugosidade nos blocos.<\/p><p>A FIGURA 3 mostra os exemplos dos mapas de aprova\u00e7\u00e3o\/reprova\u00e7\u00e3o gerados pelo software de an\u00e1lise com base em diferentes limites de rugosidade. Os blocos de rugosidade s\u00e3o destacados em vermelho quando a rugosidade da superf\u00edcie est\u00e1 acima de um determinado valor limite definido. Isso fornece uma ferramenta para o usu\u00e1rio configurar um limite de rugosidade para determinar a qualidade do acabamento da superf\u00edcie de uma amostra.<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-inner-column elementor-element elementor-element-07ce4cc\" data-id=\"07ce4cc\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-11ede0a elementor-widget elementor-widget-image\" data-id=\"11ede0a\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img decoding=\"async\" width=\"611\" height=\"455\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2023\/05\/Roughness-Standard-NANOVEA-Profilometer.jpg\" class=\"attachment-large size-large wp-image-22023\" alt=\"\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-033136d elementor-widget elementor-widget-text-editor\" data-id=\"033136d\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p style=\"text-align: center;\"><span class=\"fontstyle0\" style=\"color: #1b96cf;\">FIGURA 1:<\/span><span class=\"fontstyle0\" style=\"color: #1b96cf;\"><span style=\"color: #000000;\"><span class=\"fontstyle0\"> Varredura do sensor de linha \u00f3ptica na amostra Roughness Standard<br \/><\/span><\/span><\/span><\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-0350dcd elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"0350dcd\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-8c9ae0b\" data-id=\"8c9ae0b\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<section class=\"elementor-section elementor-inner-section elementor-element elementor-element-e08830d elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"e08830d\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-inner-column elementor-element elementor-element-d34b077\" data-id=\"d34b077\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-d015504 elementor-widget elementor-widget-text-editor\" data-id=\"d015504\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p style=\"text-align: center;\"><span class=\"fontstyle0\" style=\"color: #1b96cf;\">a.<\/span><span class=\"fontstyle0\" style=\"color: #1b96cf;\"><span style=\"color: #000000;\"><span class=\"fontstyle0\"> Mapa de altura da superf\u00edcie:<br \/><\/span><\/span><\/span><\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-3513096 elementor-widget elementor-widget-image\" data-id=\"3513096\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img loading=\"lazy\" decoding=\"async\" width=\"631\" height=\"517\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2023\/05\/Surface-Height-Map-NANOVEA-Profilometer.jpg\" class=\"attachment-large size-large wp-image-22024\" alt=\"\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-inner-column elementor-element elementor-element-82823a4\" data-id=\"82823a4\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-b85e1d4 elementor-widget elementor-widget-text-editor\" data-id=\"b85e1d4\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p style=\"text-align: center;\"><span class=\"fontstyle0\" style=\"color: #1b96cf;\">b.<\/span><span class=\"fontstyle0\" style=\"color: #1b96cf;\"><span style=\"color: #000000;\"><span class=\"fontstyle0\">\u00a0Mapa de rugosidade:<br \/><\/span><\/span><\/span><\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-8be31d3 elementor-widget elementor-widget-image\" data-id=\"8be31d3\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img loading=\"lazy\" decoding=\"async\" width=\"613\" height=\"517\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2023\/05\/Roughness-Map-NANOVEA-Profilom.jpg\" class=\"attachment-large size-large wp-image-22030\" alt=\"\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<div class=\"elementor-element elementor-element-b45ad70 elementor-widget elementor-widget-text-editor\" data-id=\"b45ad70\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p style=\"text-align: center;\"><span class=\"fontstyle0\" style=\"color: #1b96cf;\">FIGURA 2:<\/span><span class=\"fontstyle0\" style=\"color: #000000;\"> Visualiza\u00e7\u00f5es em falsa cor do mapa de altura da superf\u00edcie e do mapa de distribui\u00e7\u00e3o de rugosidade da amostra padr\u00e3o de rugosidade.<\/span><\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<section class=\"elementor-section elementor-inner-section elementor-element elementor-element-8633537 elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"8633537\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-inner-column elementor-element elementor-element-c30cd63\" data-id=\"c30cd63\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-18c70ab elementor-widget elementor-widget-image\" data-id=\"18c70ab\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img loading=\"lazy\" decoding=\"async\" width=\"380\" height=\"346\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2023\/05\/In-Line-Roughness-Inspection.jpg\" class=\"attachment-large size-large wp-image-22025\" alt=\"\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-inner-column elementor-element elementor-element-a1d8def\" data-id=\"a1d8def\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-4fcb6be elementor-widget elementor-widget-image\" data-id=\"4fcb6be\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img loading=\"lazy\" decoding=\"async\" width=\"380\" height=\"346\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2023\/05\/Roughness-Inspection-Profilometer.jpg\" class=\"attachment-large size-large wp-image-22029\" alt=\"\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<div class=\"elementor-element elementor-element-3532980 elementor-widget elementor-widget-text-editor\" data-id=\"3532980\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p style=\"text-align: center;\"><span class=\"fontstyle0\" style=\"color: #1b96cf;\">FIGURA 3:<\/span><span class=\"fontstyle0\" style=\"color: #000000;\"> Mapa de aprova\u00e7\u00e3o\/reprova\u00e7\u00e3o com base no limite de rugosidade.<\/span><\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-6b6f277 elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"6b6f277\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-no\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-00cf242\" data-id=\"00cf242\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-3a1e64a elementor-widget elementor-widget-text-editor\" data-id=\"3a1e64a\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p style=\"text-align: left;\">Inspe\u00e7\u00e3o da superf\u00edcie de uma amostra de teflon com defeitos<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-f569e54 elementor-widget elementor-widget-text-editor\" data-id=\"f569e54\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p style=\"text-align: left;\">O Mapa de Altura da Superf\u00edcie, o Mapa de Distribui\u00e7\u00e3o de Rugosidade e o Mapa de Limite de Rugosidade Aprovado\/Reprovado da superf\u00edcie da amostra Teflon s\u00e3o mostrados na FIGURA 4. A amostra de Teflon tem uma forma de cume no centro direito da amostra, conforme mostrado no mapa de altura da superf\u00edcie.<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<section class=\"elementor-section elementor-inner-section elementor-element elementor-element-19db1da elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"19db1da\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-no\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-inner-column elementor-element elementor-element-29b89d4\" data-id=\"29b89d4\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-a1185d9 elementor-widget elementor-widget-text-editor\" data-id=\"a1185d9\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p style=\"text-align: center;\"><span class=\"fontstyle0\" style=\"color: #1b96cf;\">a.<\/span><span class=\"fontstyle0\" style=\"color: #1b96cf;\"><span style=\"color: #000000;\"><span class=\"fontstyle0\"> Mapa de altura da superf\u00edcie:<br \/><\/span><\/span><\/span><\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-84d0d2a elementor-widget elementor-widget-image\" data-id=\"84d0d2a\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img loading=\"lazy\" decoding=\"async\" width=\"473\" height=\"253\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2023\/05\/NANOVEA-Profilometer-Surface-Height-Map.jpg\" class=\"attachment-large size-large wp-image-22027\" alt=\"\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-inner-column elementor-element elementor-element-6e4b370\" data-id=\"6e4b370\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-e5ebab2 elementor-widget elementor-widget-text-editor\" data-id=\"e5ebab2\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p style=\"text-align: left;\">As diferentes cores na paleta da FIGURA 4b representam o valor da rugosidade na superf\u00edcie local. O mapa de rugosidade exibe uma rugosidade homog\u00eanea na \u00e1rea intacta da amostra de Teflon. No entanto, os defeitos, na forma de um anel recuado e uma cicatriz de desgaste, s\u00e3o destacados em cores vivas. O usu\u00e1rio pode configurar facilmente um limite de rugosidade de Aprovado\/Reprovado para localizar os defeitos de superf\u00edcie, conforme mostrado na FIGURA 4c. Essa ferramenta permite aos usu\u00e1rios monitorar in situ a qualidade da superf\u00edcie do produto na linha de produ\u00e7\u00e3o e descobrir produtos defeituosos a tempo. O valor de rugosidade em tempo real \u00e9 calculado e registrado \u00e0 medida que os produtos passam pelo sensor \u00f3ptico em linha, o que pode servir como uma ferramenta r\u00e1pida e confi\u00e1vel para o controle de qualidade.<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-b21423a elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"b21423a\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-909bf4e\" data-id=\"909bf4e\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<section class=\"elementor-section elementor-inner-section elementor-element elementor-element-ccca2bd elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"ccca2bd\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-inner-column elementor-element elementor-element-d1f4c48\" data-id=\"d1f4c48\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-84625cc elementor-widget elementor-widget-text-editor\" data-id=\"84625cc\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p style=\"text-align: center;\"><span class=\"fontstyle0\" style=\"color: #1b96cf;\">b.<\/span><span class=\"fontstyle0\" style=\"color: #1b96cf;\"><span style=\"color: #000000;\"><span class=\"fontstyle0\">\u00a0Mapa de rugosidade:<br \/><\/span><\/span><\/span><\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-036926a elementor-widget elementor-widget-image\" data-id=\"036926a\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img loading=\"lazy\" decoding=\"async\" width=\"523\" height=\"284\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2023\/05\/NANOVEA-Profiler-Roughness-Map.jpg\" class=\"attachment-large size-large wp-image-22026\" alt=\"\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-inner-column elementor-element elementor-element-4a76733\" data-id=\"4a76733\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-600fa17 elementor-widget elementor-widget-text-editor\" data-id=\"600fa17\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p style=\"text-align: center;\"><span class=\"fontstyle0\" style=\"color: #1b96cf;\">c.<\/span><span class=\"fontstyle0\" style=\"color: #1b96cf;\"><span style=\"color: #000000;\"><span class=\"fontstyle0\"> Mapa de limiar de rugosidade de aprova\u00e7\u00e3o\/reprova\u00e7\u00e3o:<br \/><\/span><\/span><\/span><\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-4769e2d elementor-widget elementor-widget-image\" data-id=\"4769e2d\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img loading=\"lazy\" decoding=\"async\" width=\"472\" height=\"275\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2023\/05\/Profilometer-Roughness-Inspection-NANOVEA.jpg\" class=\"attachment-large size-large wp-image-22028\" alt=\"\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<div class=\"elementor-element elementor-element-fec470f elementor-widget elementor-widget-text-editor\" data-id=\"fec470f\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p style=\"text-align: center;\"><span class=\"fontstyle0\" style=\"color: #1b96cf;\">FIGURA 4:<\/span><span class=\"fontstyle0\" style=\"color: #000000;\"> Mapa de altura da superf\u00edcie, mapa de distribui\u00e7\u00e3o de rugosidade e <\/span><span class=\"fontstyle0\" style=\"color: #000000;\">Mapa de limiar de rugosidade de aprova\u00e7\u00e3o\/reprova\u00e7\u00e3o da superf\u00edcie da amostra do Teflon.<\/span><\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-c8c9bdf elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"c8c9bdf\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-724e51f\" data-id=\"724e51f\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-ec6977f elementor-widget elementor-widget-heading\" data-id=\"ec6977f\" data-element_type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\">CONCLUS\u00c3O<\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<section class=\"elementor-section elementor-inner-section elementor-element elementor-element-0054b85 elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"0054b85\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-inner-column elementor-element elementor-element-63eb1b9\" data-id=\"63eb1b9\" data-element_type=\"column\" data-settings=\"{&quot;background_background&quot;:&quot;classic&quot;}\">\n\t\t\t<div class=\"elementor-widget-wrap\">\n\t\t\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-inner-column elementor-element elementor-element-032d0cc\" data-id=\"032d0cc\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-dcde8ed elementor-widget elementor-widget-text-editor\" data-id=\"dcde8ed\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p>Nessa aplica\u00e7\u00e3o, mostramos como o NANOVEA ST400 3D Non-Contact Optical Profiler equipado com um sensor de linha \u00f3ptica funciona como uma ferramenta confi\u00e1vel de controle de qualidade de maneira eficaz e eficiente.<\/p><p>O sensor de linha \u00f3ptica gera uma linha brilhante de 192 pontos que escaneiam a superf\u00edcie da amostra ao mesmo tempo, o que resulta em um aumento significativo da velocidade de escaneamento. Ele pode ser instalado na linha de produ\u00e7\u00e3o para monitorar a rugosidade da superf\u00edcie dos produtos in situ. O limite de rugosidade funciona como um crit\u00e9rio confi\u00e1vel para determinar a qualidade da superf\u00edcie dos produtos, permitindo que os usu\u00e1rios percebam os produtos defeituosos a tempo.<\/p><p>Os dados mostrados aqui representam apenas uma parte dos c\u00e1lculos dispon\u00edveis no software de an\u00e1lise. Os Profil\u00f4metros NANOVEA medem praticamente qualquer superf\u00edcie em campos como Semicondutores, Microeletr\u00f4nica, Solar, Fibra \u00d3tica, Automotivo, Aeroespacial, Metalurgia, Usinagem, Revestimentos, Farmac\u00eautico, Biom\u00e9dico, Ambiental e muitos outros.<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-2dca3d1 elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"2dca3d1\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-f49c85e\" data-id=\"f49c85e\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-46aef33 elementor-widget elementor-widget-heading\" data-id=\"46aef33\" data-element_type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\">Tem um aplicativo semelhante?<\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-2ef7ed3 elementor-align-justify open-chat elementor-widget elementor-widget-button\" data-id=\"2ef7ed3\" data-element_type=\"widget\" data-widget_type=\"button.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<div class=\"elementor-button-wrapper\">\n\t\t\t\t\t<a class=\"elementor-button elementor-size-sm\" role=\"button\">\n\t\t\t\t\t\t<span class=\"elementor-button-content-wrapper\">\n\t\t\t\t\t\t\t\t\t<span class=\"elementor-button-text\">CONVERSE COM UM ESPECIALISTA AGORA<\/span>\n\t\t\t\t\t<\/span>\n\t\t\t\t\t<\/a>\n\t\t\t\t<\/div>\n\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-5ac1ba6 elementor-align-justify button-quote elementor-widget elementor-widget-button\" data-id=\"5ac1ba6\" data-element_type=\"widget\" data-widget_type=\"button.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<div class=\"elementor-button-wrapper\">\n\t\t\t\t\t<a class=\"elementor-button elementor-button-link elementor-size-sm\" href=\"https:\/\/nanovea.com\/contact-sales-form\/\" id=\"button-quote-bottom\">\n\t\t\t\t\t\t<span class=\"elementor-button-content-wrapper\">\n\t\t\t\t\t\t\t\t\t<span class=\"elementor-button-text\">OBTENHA PRE\u00c7OS E DETALHES RAPIDAMENTE<\/span>\n\t\t\t\t\t<\/span>\n\t\t\t\t\t<\/a>\n\t\t\t\t<\/div>\n\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<\/div>","protected":false},"excerpt":{"rendered":"<p>ROUGHNESS MAPPING INSPECTION USING 3D PROFILOMETRY Prepared by DUANJIE, PhD INTRODUCTION Surface roughness and texture are critical factors that impact the final quality and performance of a product. A thorough understanding of surface roughness, texture, and consistency is essential for selecting the best processing and control measures. Fast, quantifiable, and reliable inline inspection of product [&hellip;]<\/p>\n","protected":false},"author":1,"featured_media":22037,"comment_status":"open","ping_status":"open","sticky":false,"template":"","format":"standard","meta":{"_exactmetrics_skip_tracking":false,"_exactmetrics_sitenote_active":false,"_exactmetrics_sitenote_note":"","_exactmetrics_sitenote_category":0,"footnotes":""},"categories":[7,349,354,351,355,335],"tags":[],"class_list":["post-22017","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-application-notes","category-laboratory-testing","category-profilometry-flatness-warpage","category-profilometry-roughness-finish","category-profilometry-volume-area","category-profilometry-testing"],"_links":{"self":[{"href":"https:\/\/nanovea.com\/pt\/wp-json\/wp\/v2\/posts\/22017","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/nanovea.com\/pt\/wp-json\/wp\/v2\/posts"}],"about":[{"href":"https:\/\/nanovea.com\/pt\/wp-json\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"https:\/\/nanovea.com\/pt\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/nanovea.com\/pt\/wp-json\/wp\/v2\/comments?post=22017"}],"version-history":[{"count":22,"href":"https:\/\/nanovea.com\/pt\/wp-json\/wp\/v2\/posts\/22017\/revisions"}],"predecessor-version":[{"id":24693,"href":"https:\/\/nanovea.com\/pt\/wp-json\/wp\/v2\/posts\/22017\/revisions\/24693"}],"wp:featuredmedia":[{"embeddable":true,"href":"https:\/\/nanovea.com\/pt\/wp-json\/wp\/v2\/media\/22037"}],"wp:attachment":[{"href":"https:\/\/nanovea.com\/pt\/wp-json\/wp\/v2\/media?parent=22017"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"https:\/\/nanovea.com\/pt\/wp-json\/wp\/v2\/categories?post=22017"},{"taxonomy":"post_tag","embeddable":true,"href":"https:\/\/nanovea.com\/pt\/wp-json\/wp\/v2\/tags?post=22017"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}