{"id":12937,"date":"2021-08-17T17:51:03","date_gmt":"2021-08-17T17:51:03","guid":{"rendered":"https:\/\/nanovea.com\/?p=12937"},"modified":"2025-05-22T20:38:40","modified_gmt":"2025-05-22T20:38:40","slug":"aderencia-propriedades-de-revestimento-de-ouro-sobre-quartzo-cristal-substrato","status":"publish","type":"post","link":"https:\/\/nanovea.com\/pt\/adhesion-properties-of-gold-coating-on-quartz-crystal-substrate\/","title":{"rendered":"Propriedades de ades\u00e3o de revestimento de ouro sobre substrato de cristal de quartzo"},"content":{"rendered":"<div data-elementor-type=\"wp-post\" data-elementor-id=\"12937\" class=\"elementor elementor-12937\" data-elementor-post-type=\"post\">\n\t\t\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-7ec3d48 elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"7ec3d48\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-c477953\" data-id=\"c477953\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-cec2c6e elementor-widget elementor-widget-heading\" data-id=\"cec2c6e\" data-element_type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\">Propriedades de ader\u00eancia do revestimento de ouro<\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-d107f9b elementor-widget elementor-widget-heading\" data-id=\"d107f9b\" data-element_type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\"><span>sobre Substrato de Cristal de Quartzo<\/span><\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-73c118d elementor-widget elementor-widget-image\" data-id=\"73c118d\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img fetchpriority=\"high\" decoding=\"async\" width=\"768\" height=\"242\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2021\/08\/Quartz-Crystal-Microbalance-QCM-in-Vacuum-.jpg\" class=\"attachment-medium_large size-medium_large wp-image-12929\" alt=\"\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-97cc106 elementor-widget elementor-widget-heading\" data-id=\"97cc106\" data-element_type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\">Preparado por<\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-95aa94e elementor-widget elementor-widget-heading\" data-id=\"95aa94e\" data-element_type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\"><span>DUANJIE LI<\/span><span style=\"font-size:17pt\">PhD <\/span><span><\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-753c1f3 elementor-section-content-middle elementor-reverse-mobile elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"753c1f3\" data-element_type=\"section\" data-settings=\"{&quot;background_background&quot;:&quot;classic&quot;}\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-top-column elementor-element elementor-element-f2074e4\" data-id=\"f2074e4\" data-element_type=\"column\" data-settings=\"{&quot;background_background&quot;:&quot;classic&quot;}\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-c53ea2a elementor-widget elementor-widget-spacer\" data-id=\"c53ea2a\" data-element_type=\"widget\" data-widget_type=\"spacer.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t<div class=\"elementor-spacer\">\n\t\t\t<div class=\"elementor-spacer-inner\"><\/div>\n\t\t<\/div>\n\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-top-column elementor-element elementor-element-b259d86\" data-id=\"b259d86\" data-element_type=\"column\" data-settings=\"{&quot;background_background&quot;:&quot;classic&quot;}\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-62f2a44 elementor-widget elementor-widget-heading\" data-id=\"62f2a44\" data-element_type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\">INTRODU\u00c7\u00c3O<\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-9ab0009 elementor-widget elementor-widget-text-editor\" data-id=\"9ab0009\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p><span class=\"fontstyle0\">A Microbalan\u00e7a de Cristal de Quartzo (QCM) \u00e9 um sensor de massa extremamente sens\u00edvel capaz de fazer medi\u00e7\u00f5es precisas de pequena massa na faixa de nanogramas. O QCM mede a varia\u00e7\u00e3o de massa na superf\u00edcie atrav\u00e9s da detec\u00e7\u00e3o de varia\u00e7\u00f5es na freq\u00fc\u00eancia de resson\u00e2ncia do cristal de quartzo com dois eletrodos afixados em cada lado da placa. A capacidade de medir peso extremamente pequeno o torna um componente chave em uma variedade de instrumentos industriais e de pesquisa para detectar e monitorar a varia\u00e7\u00e3o de massa, adsor\u00e7\u00e3o, densidade e corros\u00e3o, etc.<\/span><\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-c9a07fb elementor-widget elementor-widget-heading\" data-id=\"c9a07fb\" data-element_type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\">IMPORT\u00c2NCIA DO TESTE DE RASPAGEM PARA QCM<\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-e74abb9 elementor-widget elementor-widget-text-editor\" data-id=\"e74abb9\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p><span class=\"fontstyle0\">Como um dispositivo extremamente preciso, o QCM mede a mudan\u00e7a de massa at\u00e9 0,1 nanograma. Qualquer perda de massa ou delamina\u00e7\u00e3o dos eletrodos na placa de quartzo ser\u00e1 detectada pelo cristal de quartzo e causar\u00e1 erros de medi\u00e7\u00e3o significativos. Como resultado, a qualidade intr\u00ednseca do revestimento do eletrodo e a integridade interfacial do sistema de revestimento\/substrato desempenham um papel essencial na realiza\u00e7\u00e3o de medi\u00e7\u00f5es de massa precisas e repet\u00edveis. O teste de micro-risco \u00e9 uma medida comparativa amplamente utilizada para avaliar a coes\u00e3o relativa ou propriedades de ades\u00e3o de revestimentos com base na compara\u00e7\u00e3o das cargas cr\u00edticas nas quais as falhas aparecem. \u00c9 uma ferramenta superior para o controle de qualidade confi\u00e1vel dos QCMs.<\/span><\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-bbe0c25 elementor-reverse-mobile elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"bbe0c25\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-5bda47b\" data-id=\"5bda47b\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<section class=\"elementor-section elementor-inner-section elementor-element elementor-element-5986dd7 elementor-reverse-mobile elementor-section-full_width elementor-reverse-tablet elementor-section-height-default elementor-section-height-default\" data-id=\"5986dd7\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-no\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-inner-column elementor-element elementor-element-77e62ae\" data-id=\"77e62ae\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-ae83510 elementor-widget elementor-widget-text-editor\" data-id=\"ae83510\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p>OBJETIVO DA MEDI\u00c7\u00c3O<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-5556e11 elementor-widget elementor-widget-text-editor\" data-id=\"5556e11\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p><em><span class=\"fontstyle0\">Nesta aplica\u00e7\u00e3o, o <\/span><span class=\"fontstyle2\">NANOVEA <\/span><span class=\"fontstyle0\"><a href=\"https:\/\/nanovea.com\/mechanical-testers\/\">Testador Mec\u00e2nico<\/a>, no modo Micro Scratch, \u00e9 usado para avaliar a for\u00e7a coesiva e adesiva do revestimento de ouro no substrato de quartzo de uma amostra QCM. Gostar\u00edamos de mostrar a capacidade do\u00a0<\/span><span class=\"fontstyle2\">NANOVEA <\/span><span class=\"fontstyle0\">Testador mec\u00e2nico na realiza\u00e7\u00e3o de testes de micro-risco em uma amostra delicada com alta precis\u00e3o e repetibilidade.<\/span><\/em><\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-34fc6f9 elementor-widget elementor-widget-spacer\" data-id=\"34fc6f9\" data-element_type=\"widget\" data-widget_type=\"spacer.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t<div class=\"elementor-spacer\">\n\t\t\t<div class=\"elementor-spacer-inner\"><\/div>\n\t\t<\/div>\n\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-7429702 elementor-widget elementor-widget-text-editor\" data-id=\"7429702\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p>NANOVEA<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-fda08d7 elementor-widget elementor-widget-text-editor\" data-id=\"fda08d7\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p>PB1000<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-inner-column elementor-element elementor-element-a6b67e5\" data-id=\"a6b67e5\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-911a059 elementor-widget elementor-widget-image\" data-id=\"911a059\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<a href=\"https:\/\/nanovea.com\/instruments\/pb1000\/\">\n\t\t\t\t\t\t\t<img decoding=\"async\" width=\"750\" height=\"804\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2020\/12\/Nanovea-PB1000-scratch-test-and-indentation.png\" class=\"elementor-animation-grow attachment-medium_large size-medium_large wp-image-9934\" alt=\"nanoindenter e testador de arranh\u00f5es Nanovea PB1000\" \/>\t\t\t\t\t\t\t\t<\/a>\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-8ec771e elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"8ec771e\" data-element_type=\"section\" data-settings=\"{&quot;background_background&quot;:&quot;classic&quot;}\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-4eba72c\" data-id=\"4eba72c\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-fbdd647 elementor-widget elementor-widget-text-editor\" data-id=\"fbdd647\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\tCONDI\u00c7\u00d5ES DE TESTE\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-21f4edc elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"21f4edc\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-fbf6d1c\" data-id=\"fbf6d1c\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-ffed5c4 elementor-widget elementor-widget-text-editor\" data-id=\"ffed5c4\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p><span class=\"fontstyle0\">O <\/span><span class=\"fontstyle2\">NANOVEA <\/span><span class=\"fontstyle0\">O Testador Mec\u00e2nico PB1000 foi usado para realizar os testes de micro-risco em uma amostra de QCM usando os par\u00e2metros de teste resumidos abaixo. Tr\u00eas arranh\u00f5es foram realizados para garantir a reprodutibilidade dos resultados.<\/span><\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-e8024a2 elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"e8024a2\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-top-column elementor-element elementor-element-685c230\" data-id=\"685c230\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-9f93ca9 elementor-widget elementor-widget-text-editor\" data-id=\"9f93ca9\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p style=\"text-align: center;\"><em><strong><span class=\"fontstyle0\" style=\"color: #1b96cf;\">TIPO CARREGADO: <\/span><span class=\"fontstyle0\" style=\"color: #000000;\">Progressivo<\/span><\/strong><\/em><\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<section class=\"elementor-section elementor-inner-section elementor-element elementor-element-fa81317 elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"fa81317\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-inner-column elementor-element elementor-element-5b718c7\" data-id=\"5b718c7\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-53be143 elementor-widget elementor-widget-text-editor\" data-id=\"53be143\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p style=\"text-align: center;\"><em><strong><span class=\"fontstyle0\">CARGA INICIAL<\/span><\/strong><\/em><\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-2191a4c elementor-widget elementor-widget-text-editor\" data-id=\"2191a4c\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p style=\"text-align: center;\"><em><strong> <span class=\"fontstyle0\">0.01 N<\/span> <\/strong><\/em><\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-inner-column elementor-element elementor-element-afbc589\" data-id=\"afbc589\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-9fbbdcb elementor-widget elementor-widget-text-editor\" data-id=\"9fbbdcb\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p style=\"text-align: center;\"><em><strong><span class=\"fontstyle0\">CARGA FINAL<\/span><\/strong><\/em><\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-d1983dc elementor-widget elementor-widget-text-editor\" data-id=\"d1983dc\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p style=\"text-align: center;\"><em><strong> <span class=\"fontstyle0\">30 N<\/span> <\/strong><\/em><\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-top-column elementor-element elementor-element-eb56f00\" data-id=\"eb56f00\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-4ba3333 elementor-widget elementor-widget-text-editor\" data-id=\"4ba3333\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p style=\"text-align: center;\"><em><strong><span class=\"fontstyle0\" style=\"color: #1b96cf;\">ATMOSPHERE: <\/span><span class=\"fontstyle0\" style=\"color: #000000;\">Ar 24\u00b0C<\/span><\/strong><\/em><\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<section class=\"elementor-section elementor-inner-section elementor-element elementor-element-6684f18 elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"6684f18\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-inner-column elementor-element elementor-element-8a90f94\" data-id=\"8a90f94\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-bac754a elementor-widget elementor-widget-text-editor\" data-id=\"bac754a\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p style=\"text-align: center;\"><em><strong><span class=\"fontstyle0\">VELOCIDADE DE DESLIZAMENTO<\/span><\/strong><\/em><\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-e36fe1a elementor-widget elementor-widget-text-editor\" data-id=\"e36fe1a\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p style=\"text-align: center;\"><em><strong> <span class=\"fontstyle0\">2 mm\/min<\/span> <\/strong><\/em><\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-inner-column elementor-element elementor-element-5be0a20\" data-id=\"5be0a20\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-c2ed58f elementor-widget elementor-widget-text-editor\" data-id=\"c2ed58f\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p style=\"text-align: center;\"><em><strong><span class=\"fontstyle0\">DIST\u00c2NCIA DE DESLIZAMENTO<\/span><\/strong><\/em><\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-818b303 elementor-widget elementor-widget-text-editor\" data-id=\"818b303\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p style=\"text-align: center;\"><em><strong> <span class=\"fontstyle0\">2 mm<\/span> <\/strong><\/em><\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-6049477 elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"6049477\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-b4cd5d7\" data-id=\"b4cd5d7\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-e68df26 elementor-widget elementor-widget-image\" data-id=\"e68df26\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img decoding=\"async\" width=\"768\" height=\"289\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2021\/08\/Rockwell-Indenter-Cone-Materials-Testing.jpg\" class=\"attachment-medium_large size-medium_large wp-image-12932\" alt=\"\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-fe841c6 elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"fe841c6\" data-element_type=\"section\" data-settings=\"{&quot;background_background&quot;:&quot;classic&quot;}\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-b7a4564\" data-id=\"b7a4564\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-47cc7e1 elementor-widget elementor-widget-text-editor\" data-id=\"47cc7e1\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\tRESULTADOS &amp; DISCUSS\u00c3O\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-5f29398 elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"5f29398\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-5b1376a\" data-id=\"5b1376a\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-eca2e19 elementor-widget elementor-widget-text-editor\" data-id=\"eca2e19\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p><span style=\"color: #000000; font-size: 16px;\">A faixa completa de micro-riscas na amostra de QCM \u00e9 mostrada em <\/span>FIGURA 1<span style=\"color: #000000; font-size: 16px;\">. Os comportamentos de falha em diferentes cargas cr\u00edticas s\u00e3o exibidos no FIGURA 2<span style=\"color: #000000; font-size: 16px;\">onde a carga cr\u00edtica, L<span style=\"color: #000000; font-size: 10px;\">C1<\/span><span style=\"color: #000000; font-size: 16px;\"> \u00e9 definida como a carga na qual o primeiro sinal de falha do adesivo ocorre na pista de raspagem, L<span style=\"color: #000000; font-size: 10px;\">C2<\/span><span style=\"color: #000000; font-size: 16px;\"> \u00e9 a carga ap\u00f3s a qual ocorrem falhas repetitivas do adesivo, e L<span style=\"color: #000000; font-size: 10px;\">C3<\/span><span style=\"color: #000000; font-size: 16px;\"> \u00e9 a carga na qual o revestimento \u00e9 completamente removido do substrato. Pode-se observar que a pequena lasca ocorre em L<span style=\"color: #000000; font-size: 10px;\">C1<\/span><span style=\"color: #000000; font-size: 16px;\"> de 11,15 N, o primeiro sinal de falha do revestimento.\u00a0<\/span><\/span><\/span><\/span><\/span><\/span><\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<section class=\"elementor-section elementor-inner-section elementor-element elementor-element-3033ed1 elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"3033ed1\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-inner-column elementor-element elementor-element-c708c82\" data-id=\"c708c82\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-e9779ed elementor-widget elementor-widget-text-editor\" data-id=\"e9779ed\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p><span style=\"color: #000000; font-size: 16px;\">Como a carga normal continua a aumentar durante o teste de micro-risco, falhas repetitivas do adesivo ocorrem ap\u00f3s o L<\/span><span style=\"color: #000000; font-size: 10px;\">C2<\/span><span style=\"color: #000000; font-size: 16px;\">\u00a0de 16,29 N. Quando L<\/span><span style=\"color: #000000; font-size: 10px;\">C3<\/span><span style=\"color: #000000; font-size: 16px;\">\u00a0de 19,09 N \u00e9 alcan\u00e7ado, o revestimento delaminates completamente do substrato de quartzo. Tais cargas cr\u00edticas podem ser usadas para comparar quantitativamente a resist\u00eancia coesiva e adesiva do revestimento e selecionar o melhor candidato para aplica\u00e7\u00f5es espec\u00edficas.<\/span><\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-inner-column elementor-element elementor-element-9667c2c\" data-id=\"9667c2c\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-112bc57 elementor-widget elementor-widget-image\" data-id=\"112bc57\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img loading=\"lazy\" decoding=\"async\" width=\"500\" height=\"306\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2021\/08\/Quartz-Crystal-Microbalance-QCM-Testing.jpg\" class=\"attachment-large size-large wp-image-12931\" alt=\"\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-b8e9638 elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"b8e9638\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-efed3fb\" data-id=\"efed3fb\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-6a76e24 elementor-widget elementor-widget-image\" data-id=\"6a76e24\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img loading=\"lazy\" decoding=\"async\" width=\"1024\" height=\"141\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2021\/08\/Micro-Scratch-Track-on-QCM.jpg\" class=\"attachment-large size-large wp-image-12926\" alt=\"\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-d74144d elementor-widget elementor-widget-text-editor\" data-id=\"d74144d\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p style=\"text-align: center;\"><span class=\"fontstyle0\" style=\"color: #1b96cf;\">FIGURA 1: <\/span><span class=\"fontstyle0\" style=\"color: #000000;\">Pista de micro arranh\u00f5es completa na amostra do QCM.<\/span><\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<section class=\"elementor-section elementor-inner-section elementor-element elementor-element-a6f671e elementor-section-content-top elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"a6f671e\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-33 elementor-inner-column elementor-element elementor-element-d9e612f\" data-id=\"d9e612f\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-e5eb952 elementor-widget elementor-widget-image\" data-id=\"e5eb952\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img decoding=\"async\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2021\/08\/Micro-scratch-track-Mechanical-Tester.png\" title=\"\" alt=\"\" loading=\"lazy\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t<div class=\"elementor-column elementor-col-33 elementor-inner-column elementor-element elementor-element-df357c5\" data-id=\"df357c5\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-607f575 elementor-widget elementor-widget-image\" data-id=\"607f575\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img decoding=\"async\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2021\/08\/Micro-scratch-track-NANOVEA.png\" title=\"\" alt=\"\" loading=\"lazy\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t<div class=\"elementor-column elementor-col-33 elementor-inner-column elementor-element elementor-element-daafcbf\" data-id=\"daafcbf\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-b1e8978 elementor-widget elementor-widget-image\" data-id=\"b1e8978\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img decoding=\"async\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2021\/08\/Micro-scratch-track-Materials-Testing.png\" title=\"\" alt=\"\" loading=\"lazy\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<div class=\"elementor-element elementor-element-2f63726 elementor-widget elementor-widget-text-editor\" data-id=\"2f63726\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p style=\"text-align: center;\"><span class=\"fontstyle0\" style=\"color: #1b96cf;\">FIGURA 2: <\/span><span class=\"fontstyle0\" style=\"color: #000000;\">Micro raspador em diferentes cargas cr\u00edticas.<\/span><\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-28aa079 elementor-widget elementor-widget-text-editor\" data-id=\"28aa079\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p><span class=\"fontstyle0\">FIGURA 3 <\/span><span class=\"fontstyle2\">tra\u00e7a a evolu\u00e7\u00e3o do coeficiente de atrito e profundidade que pode fornecer mais informa\u00e7\u00f5es sobre a progress\u00e3o de falhas no revestimento durante o teste de micro-risco.<\/span><\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-46e6014 elementor-widget elementor-widget-image\" data-id=\"46e6014\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img loading=\"lazy\" decoding=\"async\" width=\"1024\" height=\"500\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2021\/08\/Quartz-Crystal-Microbalance-Testing-QCM.jpg\" class=\"attachment-large size-large wp-image-12930\" alt=\"\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-147e8c8 elementor-widget elementor-widget-text-editor\" data-id=\"147e8c8\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p style=\"text-align: center;\"><span class=\"fontstyle0\" style=\"color: #1b96cf;\">FIGURA 3: <\/span><span class=\"fontstyle0\" style=\"color: #000000;\">Evolu\u00e7\u00e3o do COF e Profundidade durante o teste de micro-risco.<\/span><\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-c2bb1c9 elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"c2bb1c9\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-7628b4d\" data-id=\"7628b4d\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-784c0d2 elementor-widget elementor-widget-heading\" data-id=\"784c0d2\" data-element_type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\">CONCLUS\u00c3O<\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-445fc39 elementor-widget elementor-widget-text-editor\" data-id=\"445fc39\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p><span class=\"fontstyle0\">Neste estudo, mostramos que o\u00a0<\/span><span class=\"fontstyle2\">NANOVEA <\/span><span class=\"fontstyle0\">O Testador Mec\u00e2nico realiza testes confi\u00e1veis e precisos de micro arranh\u00f5es em uma amostra de QCM. Ao aplicar cargas linearmente aumentadas de forma controlada e monitorada de perto, a medi\u00e7\u00e3o de arranh\u00f5es permite aos usu\u00e1rios identificar a carga cr\u00edtica na qual ocorre a t\u00edpica falha do revestimento coesivo e adesivo. Ela fornece uma ferramenta superior para avaliar e comparar quantitativamente a qualidade intr\u00ednseca do revestimento e a integridade interfacial do sistema de revestimento\/substrato para QCM.<\/span><\/p><p><span class=\"fontstyle0\">Os m\u00f3dulos Nano, Micro ou Macro do <\/span><span class=\"fontstyle2\">NANOVEA <\/span><span class=\"fontstyle0\">Todos os testes mec\u00e2nicos incluem indenta\u00e7\u00e3o em conformidade com ISO e ASTM, modos de teste de arranh\u00f5es e desgaste, proporcionando a maior e mais amig\u00e1vel gama de testes dispon\u00edveis em um \u00fanico sistema. <\/span><span class=\"fontstyle2\">NANOVEA<\/span><span class=\"fontstyle0\">A gama inigual\u00e1vel da Young \u00e9 uma solu\u00e7\u00e3o ideal para determinar a gama completa de propriedades mec\u00e2nicas de revestimentos finos ou grossos, macios ou duros, filmes e substratos, incluindo dureza, m\u00f3dulo Young, resist\u00eancia \u00e0 fratura, ader\u00eancia, resist\u00eancia ao desgaste e muitos outros.<\/span><\/p><p><span class=\"fontstyle0\">Al\u00e9m disso, um profiler 3D opcional sem contato e um m\u00f3dulo AFM est\u00e3o dispon\u00edveis para imagens 3D de alta resolu\u00e7\u00e3o de indenta\u00e7\u00e3o, raspagem e pista de desgaste, al\u00e9m de outras medidas de superf\u00edcie, tais como rugosidade e deforma\u00e7\u00e3o.<\/span><\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-26f60c9 elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"26f60c9\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-05e6cf9\" data-id=\"05e6cf9\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-1d0c987 elementor-widget elementor-widget-heading\" data-id=\"1d0c987\" data-element_type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\">Tem um aplicativo semelhante?<\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-534dee9 elementor-align-justify open-chat elementor-widget elementor-widget-button\" data-id=\"534dee9\" data-element_type=\"widget\" data-widget_type=\"button.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<div class=\"elementor-button-wrapper\">\n\t\t\t\t\t<a class=\"elementor-button elementor-size-sm\" role=\"button\">\n\t\t\t\t\t\t<span class=\"elementor-button-content-wrapper\">\n\t\t\t\t\t\t\t\t\t<span class=\"elementor-button-text\">CONVERSE COM UM ESPECIALISTA AGORA<\/span>\n\t\t\t\t\t<\/span>\n\t\t\t\t\t<\/a>\n\t\t\t\t<\/div>\n\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-5411243 elementor-align-justify button-quote elementor-widget elementor-widget-button\" data-id=\"5411243\" data-element_type=\"widget\" data-widget_type=\"button.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<div class=\"elementor-button-wrapper\">\n\t\t\t\t\t<a class=\"elementor-button elementor-button-link elementor-size-sm\" href=\"https:\/\/nanovea.com\/contact-sales-form\/\" id=\"button-quote-bottom\">\n\t\t\t\t\t\t<span class=\"elementor-button-content-wrapper\">\n\t\t\t\t\t\t\t\t\t<span class=\"elementor-button-text\">OBTENHA PRE\u00c7OS E DETALHES RAPIDAMENTE<\/span>\n\t\t\t\t\t<\/span>\n\t\t\t\t\t<\/a>\n\t\t\t\t<\/div>\n\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<\/div>","protected":false},"excerpt":{"rendered":"<p>Adhesion Properties of Gold Coating on Quartz Crystal Substrate Prepared by DUANJIE LI, PhD INTRODUCTION The Quartz Crystal Microbalance (QCM) is an extremely sensitive mass sensor capable of making precise measurements of small mass in the nanogram range. QCM measures the mass change on the surface through detecting variations in resonance frequency of the quartz [&hellip;]<\/p>\n","protected":false},"author":1,"featured_media":12979,"comment_status":"open","ping_status":"open","sticky":false,"template":"","format":"standard","meta":{"_exactmetrics_skip_tracking":false,"_exactmetrics_sitenote_active":false,"_exactmetrics_sitenote_note":"","_exactmetrics_sitenote_category":0,"footnotes":""},"categories":[7,349,337,345,346],"tags":[],"class_list":["post-12937","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-application-notes","category-laboratory-testing","category-mechanical-testing","category-scratch-testing-adhesive-failure","category-scratch-testing-cohesive-failure"],"_links":{"self":[{"href":"https:\/\/nanovea.com\/pt\/wp-json\/wp\/v2\/posts\/12937","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/nanovea.com\/pt\/wp-json\/wp\/v2\/posts"}],"about":[{"href":"https:\/\/nanovea.com\/pt\/wp-json\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"https:\/\/nanovea.com\/pt\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/nanovea.com\/pt\/wp-json\/wp\/v2\/comments?post=12937"}],"version-history":[{"count":47,"href":"https:\/\/nanovea.com\/pt\/wp-json\/wp\/v2\/posts\/12937\/revisions"}],"predecessor-version":[{"id":24731,"href":"https:\/\/nanovea.com\/pt\/wp-json\/wp\/v2\/posts\/12937\/revisions\/24731"}],"wp:featuredmedia":[{"embeddable":true,"href":"https:\/\/nanovea.com\/pt\/wp-json\/wp\/v2\/media\/12979"}],"wp:attachment":[{"href":"https:\/\/nanovea.com\/pt\/wp-json\/wp\/v2\/media?parent=12937"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"https:\/\/nanovea.com\/pt\/wp-json\/wp\/v2\/categories?post=12937"},{"taxonomy":"post_tag","embeddable":true,"href":"https:\/\/nanovea.com\/pt\/wp-json\/wp\/v2\/tags?post=12937"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}