{"id":6927,"date":"2019-09-04T16:59:53","date_gmt":"2019-09-04T16:59:53","guid":{"rendered":"https:\/\/nanovea.com\/?p=6927"},"modified":"2023-11-13T22:37:18","modified_gmt":"2023-11-13T22:37:18","slug":"porownanie-smarowania-oka-z-uzyciem-trymetru-nanovea-t50","status":"publish","type":"post","link":"https:\/\/nanovea.com\/pl\/lubricating-eye-drop-comparison-using-the-nanovea-t50-tribometer\/","title":{"rendered":"Por\u00f3wnanie kropli nawil\u017caj\u0105cych do oczu przy u\u017cyciu trybometru Nanovea T50"},"content":{"rendered":"<div data-elementor-type=\"wp-post\" data-elementor-id=\"6927\" class=\"elementor elementor-6927\" data-elementor-post-type=\"post\">\n\t\t\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-21cd638d elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"21cd638d\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-42ec104d\" data-id=\"42ec104d\" data-element_type=\"column\" data-settings=\"{&quot;background_background&quot;:&quot;classic&quot;}\">\n\t\t\t<div class=\"elementor-widget-wrap\">\n\t\t\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-42d11421 elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"42d11421\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-55297c0c\" data-id=\"55297c0c\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-6ba397b8 elementor-widget elementor-widget-text-editor\" data-id=\"6ba397b8\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p style=\"text-align: left; color: #1b96cf; font-size: 24px;\">Znaczenie testowania kropli do oczu<strong><u><i><br><\/i><\/u><\/strong><\/p>\n<div>Krople do oczu s\u0105 stosowane w celu z\u0142agodzenia objaw\u00f3w spowodowanych przez szereg problem\u00f3w z oczami. Mog\u0105 by\u0107 na przyk\u0142ad stosowane w leczeniu niewielkiego podra\u017cnienia oczu (np. sucho\u015bci i zaczerwienienia), op\u00f3\u017anienia wyst\u0105pienia jaskry lub leczenia infekcji. Krople do oczu sprzedawane bez recepty s\u0105 stosowane g\u0142\u00f3wnie w leczeniu sucho\u015bci. Ich skuteczno\u015b\u0107 w smarowaniu oka mo\u017cna por\u00f3wna\u0107 i zmierzy\u0107 za pomoc\u0105 testu wsp\u00f3\u0142czynnika tarcia.<\/div>\n<div>&nbsp;<\/div>\n<div>Sucho\u015b\u0107 oczu mo\u017ce by\u0107 spowodowana wieloma czynnikami, na przyk\u0142ad przem\u0119czeniem oczu przy komputerze lub przebywaniem na zewn\u0105trz w ekstremalnych warunkach pogodowych. Dobre nawil\u017caj\u0105ce krople do oczu pomagaj\u0105 utrzyma\u0107 i uzupe\u0142ni\u0107 wilgo\u0107 na zewn\u0119trznej powierzchni oczu. Dzi\u0119ki temu \u0142agodz\u0105 dyskomfort, pieczenie lub podra\u017cnienie i zaczerwienienie zwi\u0105zane z sucho\u015bci\u0105 oczu. Mierz\u0105c wsp\u00f3\u0142czynnik tarcia (COF) roztworu kropli do oczu, mo\u017cna okre\u015bli\u0107 jego skuteczno\u015b\u0107 smarowania i por\u00f3wna\u0107 go z innymi rozwi\u0105zaniami.<\/div>\n\n<p style=\"text-align: left; color: #1b96cf; font-size: 24px;\">Cel pomiaru<\/p>\n<p>W tym badaniu zmierzono wsp\u00f3\u0142czynnik tarcia (COF) trzech r\u00f3\u017cnych smaruj\u0105cych roztwor\u00f3w kropli do oczu, stosuj\u0105c uk\u0142ad pin-on-disk na tribometrze Nanovea T50.<\/p>\n<div style=\"text-align: center;\"><a href=\"https:\/\/nanovea.com\/wp-content\/uploads\/2019\/09\/Measurement-objective-picture.png\"><img fetchpriority=\"high\" decoding=\"async\" class=\"alignnone size-full wp-image-8113\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2019\/09\/Measurement-objective-picture.png\" alt=\"\" width=\"917\" height=\"649\"><\/a><\/div>\n<p style=\"text-align: left; color: #1b96cf; font-size: 24px;\">Procedura badania i procedury<strong><u><i><br><\/i><\/u><\/strong><\/p>\n<p>Kulisty trzpie\u0144 o \u015brednicy 6 mm wykonany z tlenku glinu zosta\u0142 przy\u0142o\u017cony do szklanego szkie\u0142ka, przy czym ka\u017cdy roztw\u00f3r kropli do oczu dzia\u0142a\u0142 jako \u015brodek smarny pomi\u0119dzy dwoma powierzchniami. Parametry badawcze stosowane we wszystkich eksperymentach zestawiono w tabeli 1 poni\u017cej.<\/p>\n<div style=\"text-align: center;\"><a href=\"https:\/\/nanovea.com\/wp-content\/uploads\/2019\/09\/Samples-picture.png\"><img decoding=\"async\" class=\"alignnone size-full wp-image-8114\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2019\/09\/Samples-picture.png\" alt=\"\" width=\"604\" height=\"805\"><\/a><\/div>\n<p style=\"text-align: left; color: #1b96cf; font-size: 24px;\">Wyniki i dyskusja<u><i><\/i><\/u><\/p>\n<p style=\"margin: 0in; margin-bottom: .0001pt;\"><span style=\"font-family: 'Arial',sans-serif;\">Maksymalne, minimalne i \u015brednie warto\u015bci wsp\u00f3\u0142czynnika tarcia dla trzech r\u00f3\u017cnych badanych roztwor\u00f3w kropli do oczu przedstawiono w tabeli 2 poni\u017cej. Wykresy COF v. Obroty dla ka\u017cdego roztworu kropli do oczu przedstawiono na rysunkach 2-4. Wsp\u00f3\u0142czynnik COF podczas ka\u017cdego testu pozostawa\u0142 wzgl\u0119dnie sta\u0142y przez wi\u0119kszo\u015b\u0107 ca\u0142kowitego czasu trwania testu. Pr\u00f3bka A mia\u0142a najni\u017cszy \u015bredni COF, co wskazuje na jej najlepsze w\u0142a\u015bciwo\u015bci smaruj\u0105ce.<\/span><\/p>\n<p style=\"margin: 0in; margin-bottom: .0001pt;\"><span style=\"font-family: 'Arial',sans-serif; color: #1c1e29;\">&nbsp;<\/span><\/p>\n<p><a href=\"https:\/\/nanovea.com\/wp-content\/uploads\/2019\/09\/Figure-2.png\"><img decoding=\"async\" class=\"alignnone size-full wp-image-8115\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2019\/09\/Figure-2.png\" alt=\"\" width=\"1001\" height=\"893\"><\/a><\/p>\n<p><a href=\"https:\/\/nanovea.com\/wp-content\/uploads\/2019\/09\/Figure-3.png\"><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-8116\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2019\/09\/Figure-3.png\" alt=\"\" width=\"1285\" height=\"776\"><\/a><\/p>\n<p><a href=\"https:\/\/nanovea.com\/wp-content\/uploads\/2019\/09\/Figure-4.png\"><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-8117\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2019\/09\/Figure-4.png\" alt=\"\" width=\"1267\" height=\"794\"><\/a><\/p>\n<p style=\"text-align: left; color: #1b96cf; font-size: 24px;\">Wniosek<\/p>\n<p><a href=\"https:\/\/nanovea.com\/wp-content\/uploads\/2019\/09\/CoefficientofFrictionofEyeDrop.jpg\"><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-8121\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2019\/09\/CoefficientofFrictionofEyeDrop.jpg\" alt=\"\" width=\"1216\" height=\"777\"><\/a><\/p>\n<p>W tym badaniu zaprezentowano mo\u017cliwo\u015bci Tribometru Nanovea T50 w zakresie pomiaru wsp\u00f3\u0142czynnika tarcia trzech roztwor\u00f3w kropli do oczu. Na podstawie tych warto\u015bci wykazali\u015bmy, \u017ce pr\u00f3bka A mia\u0142a ni\u017cszy wsp\u00f3\u0142czynnik tarcia i dlatego wykazywa\u0142a lepsze smarowanie w por\u00f3wnaniu do pozosta\u0142ych dw\u00f3ch pr\u00f3bek.<\/p>\n<p>Nanovea <a href=\"https:\/\/nanovea.com\/tribometers\/\">Tribometry <\/a>oferuje precyzyjne i powtarzalne badania zu\u017cycia i tarcia przy u\u017cyciu modu\u0142\u00f3w obrotowych i liniowych zgodnych z ISO i ASTM. Zapewnia tak\u017ce opcjonalne modu\u0142y zu\u017cywaj\u0105ce si\u0119 w wysokich temperaturach, smaruj\u0105ce i trybokorozyjne, dost\u0119pne w jednym, wst\u0119pnie zintegrowanym systemie. Taka wszechstronno\u015b\u0107 pozwala u\u017cytkownikom lepiej symulowa\u0107 rzeczywiste \u015brodowisko aplikacji i poprawi\u0107 podstawow\u0105 wiedz\u0119 na temat mechanizmu zu\u017cycia i w\u0142a\u015bciwo\u015bci tribologicznych r\u00f3\u017cnych materia\u0142\u00f3w.<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-2f41878 elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"2f41878\" data-element_type=\"section\" data-settings=\"{&quot;background_background&quot;:&quot;classic&quot;}\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-a6030dc\" data-id=\"a6030dc\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-acb17e4 elementor-widget elementor-widget-heading\" data-id=\"acb17e4\" data-element_type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\"><b>TERAZ POROZMAWIAJMY O TWOJEJ APLIKACJI<\/b><\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-f96103e live-chat elementor-align-center elementor-widget elementor-widget-button\" data-id=\"f96103e\" data-element_type=\"widget\" data-widget_type=\"button.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<div class=\"elementor-button-wrapper\">\n\t\t\t\t\t<a class=\"elementor-button elementor-button-link elementor-size-md\" href=\"https:\/\/nanovea.com\/contact\/live-chat\/\" id=\"live-chat\">\n\t\t\t\t\t\t<span class=\"elementor-button-content-wrapper\">\n\t\t\t\t\t\t\t\t\t<span class=\"elementor-button-text\">LIVE CHAT<\/span>\n\t\t\t\t\t<\/span>\n\t\t\t\t\t<\/a>\n\t\t\t\t<\/div>\n\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<\/div>","protected":false},"excerpt":{"rendered":"<p>Importance of Testing Eye Drop Solutions Eye drop solutions are used to alleviate symptoms caused by a range of eye problems. For example, they can be used to treat minor eye irritation (e.g. dryness and redness), delay the onset of glaucoma or treat infections. Eye drop solutions sold over-the-counter are mainly used to treat dryness. [&hellip;]<\/p>\n","protected":false},"author":1,"featured_media":6936,"comment_status":"open","ping_status":"open","sticky":false,"template":"","format":"standard","meta":{"_exactmetrics_skip_tracking":false,"_exactmetrics_sitenote_active":false,"_exactmetrics_sitenote_note":"","_exactmetrics_sitenote_category":0,"footnotes":""},"categories":[7,349,380,373,336],"tags":[],"class_list":["post-6927","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-application-notes","category-laboratory-testing","category-liquid-tribology","category-rotational-tribology","category-tribology-testing"],"_links":{"self":[{"href":"https:\/\/nanovea.com\/pl\/wp-json\/wp\/v2\/posts\/6927","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/nanovea.com\/pl\/wp-json\/wp\/v2\/posts"}],"about":[{"href":"https:\/\/nanovea.com\/pl\/wp-json\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"https:\/\/nanovea.com\/pl\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/nanovea.com\/pl\/wp-json\/wp\/v2\/comments?post=6927"}],"version-history":[{"count":17,"href":"https:\/\/nanovea.com\/pl\/wp-json\/wp\/v2\/posts\/6927\/revisions"}],"predecessor-version":[{"id":23430,"href":"https:\/\/nanovea.com\/pl\/wp-json\/wp\/v2\/posts\/6927\/revisions\/23430"}],"wp:featuredmedia":[{"embeddable":true,"href":"https:\/\/nanovea.com\/pl\/wp-json\/wp\/v2\/media\/6936"}],"wp:attachment":[{"href":"https:\/\/nanovea.com\/pl\/wp-json\/wp\/v2\/media?parent=6927"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"https:\/\/nanovea.com\/pl\/wp-json\/wp\/v2\/categories?post=6927"},{"taxonomy":"post_tag","embeddable":true,"href":"https:\/\/nanovea.com\/pl\/wp-json\/wp\/v2\/tags?post=6927"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}