{"id":2646,"date":"2016-11-29T21:21:46","date_gmt":"2016-11-29T21:21:46","guid":{"rendered":"http:\/\/nanovea.com\/?p=2646"},"modified":"2016-11-29T21:22:08","modified_gmt":"2016-11-29T21:22:08","slug":"trybologia-inspekcja","status":"publish","type":"post","link":"https:\/\/nanovea.com\/pl\/tribology-inspection\/","title":{"rendered":"Kontrola trybologiczna pow\u0142ok z azotku tytanu za pomoc\u0105 trybometru"},"content":{"rendered":"<p>Zu\u017cycie narz\u0119dzi podczas pracy powoduje utrat\u0119 wymiar\u00f3w i funkcjonalno\u015bci narz\u0119dzi. Ma to znacz\u0105cy wp\u0142yw na \u017cywotno\u015b\u0107 narz\u0119dzia, a tak\u017ce integralno\u015b\u0107 powierzchni i dok\u0142adno\u015b\u0107 wymiar\u00f3w gotowych produkt\u00f3w. W\u0142a\u015bciwo\u015bci trybologiczno-mechaniczne ceramicznych pow\u0142ok ochronnych mog\u0105 znacz\u0105co poprawi\u0107 wydajno\u015b\u0107 i \u017cywotno\u015b\u0107 obrabiarek. Niezawodna i dok\u0142adna kontrola trybologiczna takich pow\u0142ok ochronnych staje si\u0119 kluczowa dla zapewnienia wysokiej jako\u015bci dzia\u0142ania narz\u0119dzi.<\/p>\n<p><a href=\"https:\/\/nanovea.com\/App-Notes\/tribology-inspection.pdf\">Kontrola pow\u0142ok z azotku tytanu za pomoc\u0105 trybometru<\/a><\/p>","protected":false},"excerpt":{"rendered":"<p>Wear of the tools in service creates loss of dimensions and functionality of the tools. It has significant influence on the tool life, as well as the surface integrity and dimension accuracy of the finished products. The tribo-mechanical properties of the protective ceramic coatings can substantially enhance the service performance and lifespan of the machine [&hellip;]<\/p>\n","protected":false},"author":1,"featured_media":2638,"comment_status":"open","ping_status":"open","sticky":false,"template":"","format":"standard","meta":{"_exactmetrics_skip_tracking":false,"_exactmetrics_sitenote_active":false,"_exactmetrics_sitenote_note":"","_exactmetrics_sitenote_category":0,"footnotes":""},"categories":[7],"tags":[263],"class_list":["post-2646","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-application-notes","tag-tribology-inspection"],"_links":{"self":[{"href":"https:\/\/nanovea.com\/pl\/wp-json\/wp\/v2\/posts\/2646","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/nanovea.com\/pl\/wp-json\/wp\/v2\/posts"}],"about":[{"href":"https:\/\/nanovea.com\/pl\/wp-json\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"https:\/\/nanovea.com\/pl\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/nanovea.com\/pl\/wp-json\/wp\/v2\/comments?post=2646"}],"version-history":[{"count":1,"href":"https:\/\/nanovea.com\/pl\/wp-json\/wp\/v2\/posts\/2646\/revisions"}],"predecessor-version":[{"id":2647,"href":"https:\/\/nanovea.com\/pl\/wp-json\/wp\/v2\/posts\/2646\/revisions\/2647"}],"wp:featuredmedia":[{"embeddable":true,"href":"https:\/\/nanovea.com\/pl\/wp-json\/wp\/v2\/media\/2638"}],"wp:attachment":[{"href":"https:\/\/nanovea.com\/pl\/wp-json\/wp\/v2\/media?parent=2646"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"https:\/\/nanovea.com\/pl\/wp-json\/wp\/v2\/categories?post=2646"},{"taxonomy":"post_tag","embeddable":true,"href":"https:\/\/nanovea.com\/pl\/wp-json\/wp\/v2\/tags?post=2646"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}