{"id":16045,"date":"2021-11-01T20:39:55","date_gmt":"2021-11-01T20:39:55","guid":{"rendered":"https:\/\/nanovea.com\/?p=16045"},"modified":"2025-03-26T20:56:09","modified_gmt":"2025-03-26T20:56:09","slug":"papier-scierny-scieranie-wykonywanie-uzywania-tribometru","status":"publish","type":"post","link":"https:\/\/nanovea.com\/pl\/sandpaper-abrasion-performance-using-a-tribometer\/","title":{"rendered":"\u015acieralno\u015b\u0107 papieru \u015bciernego na tribometrze"},"content":{"rendered":"<div data-elementor-type=\"wp-post\" data-elementor-id=\"16045\" class=\"elementor elementor-16045\" data-elementor-post-type=\"post\">\n\t\t\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-7ec3d48 elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"7ec3d48\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-c477953\" data-id=\"c477953\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-366d50f elementor-widget elementor-widget-heading\" data-id=\"366d50f\" data-element_type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h1 class=\"elementor-heading-title elementor-size-default\">WYDAJNO\u015a\u0106 \u015aCIERANIA PAPIERU \u015aCIERNEGO<\/h1>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-d107f9b elementor-widget elementor-widget-heading\" data-id=\"d107f9b\" data-element_type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\">PRZY U\u017bYCIU TRYBOMETRU<\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-73c118d elementor-widget elementor-widget-image\" data-id=\"73c118d\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img fetchpriority=\"high\" decoding=\"async\" width=\"768\" height=\"217\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2021\/10\/Sandpaper-Abrasion-Testing-Services.jpg\" class=\"attachment-medium_large size-medium_large wp-image-16071\" alt=\"Testy \u015bcieralno\u015bci papieru \u015bciernego\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-97cc106 elementor-widget elementor-widget-heading\" data-id=\"97cc106\" data-element_type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\">Przygotowane przez<\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-95aa94e elementor-widget elementor-widget-heading\" data-id=\"95aa94e\" data-element_type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\">DUANJIE LI, PhD<\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-c14383d elementor-widget elementor-widget-spacer\" data-id=\"c14383d\" data-element_type=\"widget\" data-widget_type=\"spacer.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t<div class=\"elementor-spacer\">\n\t\t\t<div class=\"elementor-spacer-inner\"><\/div>\n\t\t<\/div>\n\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-753c1f3 elementor-section-content-middle elementor-reverse-mobile elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"753c1f3\" data-element_type=\"section\" data-settings=\"{&quot;background_background&quot;:&quot;classic&quot;}\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-top-column elementor-element elementor-element-f2074e4 elementor-hidden-phone\" data-id=\"f2074e4\" data-element_type=\"column\" data-settings=\"{&quot;background_background&quot;:&quot;classic&quot;}\">\n\t\t\t<div class=\"elementor-widget-wrap\">\n\t\t\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-top-column elementor-element elementor-element-b259d86\" data-id=\"b259d86\" data-element_type=\"column\" data-settings=\"{&quot;background_background&quot;:&quot;classic&quot;}\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-62f2a44 elementor-widget elementor-widget-heading\" data-id=\"62f2a44\" data-element_type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\">WPROWADZENIE<\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-9ab0009 elementor-widget elementor-widget-text-editor\" data-id=\"9ab0009\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p>Papier \u015bcierny sk\u0142ada si\u0119 z cz\u0105stek \u015bciernych przyklejonych do jednej strony papieru lub tkaniny. Jako cz\u0105stki mo\u017cna stosowa\u0107 r\u00f3\u017cne materia\u0142y \u015bcierne, takie jak granat, w\u0119glik krzemu, tlenek aluminium i diament. Papier \u015bcierny jest szeroko stosowany w r\u00f3\u017cnych sektorach przemys\u0142u do tworzenia specyficznych wyko\u0144cze\u0144 powierzchni na drewnie, metalu i suchej zabudowie. Cz\u0119sto pracuj\u0105 pod wysokim ci\u015bnieniem kontaktowym stosowanym przez narz\u0119dzia r\u0119czne lub elektryczne.<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-c9a07fb elementor-widget elementor-widget-heading\" data-id=\"c9a07fb\" data-element_type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h3 class=\"elementor-heading-title elementor-size-default\">ZNACZENIE OCENY WYDAJNO\u015aCI \u015aCIERANIA PAPIERU \u015aCIERNEGO<\/h3>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-e74abb9 elementor-widget elementor-widget-text-editor\" data-id=\"e74abb9\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p>Skuteczno\u015b\u0107 papieru \u015bciernego jest cz\u0119sto okre\u015blana na podstawie jego wydajno\u015bci \u015bcierania w r\u00f3\u017cnych warunkach. Wielko\u015b\u0107 ziarna, tzn. wielko\u015b\u0107 cz\u0105stek \u015bciernych osadzonych w papierze \u015bciernym, decyduje o szybko\u015bci zu\u017cycia i wielko\u015bci rys na szlifowanym materiale. Papiery \u015bcierne o wy\u017cszej granulacji maj\u0105 mniejsze cz\u0105stki, co powoduje ni\u017csze pr\u0119dko\u015bci szlifowania i drobniejsze wyko\u0144czenie powierzchni. Papiery \u015bcierne o tej samej liczbie ziarna, ale wykonane z r\u00f3\u017cnych materia\u0142\u00f3w, mog\u0105 mie\u0107 r\u00f3\u017cne zachowanie w warunkach suchych i mokrych. Aby zagwarantowa\u0107, \u017ce wyprodukowany papier \u015bcierny b\u0119dzie zachowywa\u0142 si\u0119 tak jak nale\u017cy, konieczne s\u0105 wiarygodne badania tribologiczne. Dzi\u0119ki tym badaniom mo\u017cliwe jest ilo\u015bciowe por\u00f3wnanie zu\u017cycia r\u00f3\u017cnych rodzaj\u00f3w papieru \u015bciernego w spos\u00f3b kontrolowany i monitorowany, co pozwala na wyb\u00f3r najlepszego kandydata do danego zastosowania.<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-bbe0c25 elementor-reverse-mobile elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"bbe0c25\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-5bda47b\" data-id=\"5bda47b\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<section class=\"elementor-section elementor-inner-section elementor-element elementor-element-702ad1d elementor-reverse-mobile elementor-section-full_width elementor-reverse-tablet elementor-section-height-default elementor-section-height-default\" data-id=\"702ad1d\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-no\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-inner-column elementor-element elementor-element-9623762\" data-id=\"9623762\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-267c2d8 elementor-widget elementor-widget-heading\" data-id=\"267c2d8\" data-element_type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\">CEL POMIARU<\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-fa7ad49 elementor-widget elementor-widget-text-editor\" data-id=\"fa7ad49\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p><em>W tym badaniu prezentujemy zdolno\u015b\u0107 Tribometru Pneumatycznego Wysokiego Obci\u0105\u017cenia NANOVEA T2000 do ilo\u015bciowej oceny wydajno\u015bci \u015bcierania r\u00f3\u017cnych pr\u00f3bek papieru \u015bciernego w warunkach suchych i mokrych.<\/em><\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-0efde9a elementor-widget__width-initial elementor-widget elementor-widget-text-editor\" data-id=\"0efde9a\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p style=\"text-align: center; font-size: 20pt; color: black;\">NANOVEA <span style=\"font-size: 20pt; color: #1b96cf;\">T2000 Wysokie obci\u0105\u017cenie<br \/><\/span><span style=\"font-size: 20pt;\">Trybometr pneumatyczny<\/span><\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t<div class=\"elementor-element elementor-element-29a08fb e-grid e-con-full e-con e-child\" data-id=\"29a08fb\" data-element_type=\"container\">\n\t\t\t\t<div class=\"elementor-element elementor-element-4f88fcd elementor-align-center homepage-button-brochure elementor-widget elementor-widget-button\" data-id=\"4f88fcd\" data-element_type=\"widget\" data-widget_type=\"button.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<div class=\"elementor-button-wrapper\">\n\t\t\t\t\t<a class=\"elementor-button elementor-button-link elementor-size-sm\" href=\"https:\/\/nanovea.com\/t2000-tribometer-brochure-form\/\" id=\"homepage-button-brochure\">\n\t\t\t\t\t\t<span class=\"elementor-button-content-wrapper\">\n\t\t\t\t\t\t\t\t\t<span class=\"elementor-button-text\">POBIERZ BROSZUR\u0118<\/span>\n\t\t\t\t\t<\/span>\n\t\t\t\t\t<\/a>\n\t\t\t\t<\/div>\n\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-c967855 elementor-align-center homepage-button-quote elementor-widget elementor-widget-button\" data-id=\"c967855\" data-element_type=\"widget\" data-widget_type=\"button.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<div class=\"elementor-button-wrapper\">\n\t\t\t\t\t<a class=\"elementor-button elementor-button-link elementor-size-sm\" href=\"https:\/\/nanovea.com\/contact-sales-form\/\" id=\"homepage-button-quote\">\n\t\t\t\t\t\t<span class=\"elementor-button-content-wrapper\">\n\t\t\t\t\t\t\t\t\t<span class=\"elementor-button-text\">ZADAJ PYTANIE<\/span>\n\t\t\t\t\t<\/span>\n\t\t\t\t\t<\/a>\n\t\t\t\t<\/div>\n\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-inner-column elementor-element elementor-element-c441b48\" data-id=\"c441b48\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-7e3594e elementor-widget elementor-widget-image\" data-id=\"7e3594e\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<a href=\"https:\/\/nanovea.com\/instruments\/t2000\/\">\n\t\t\t\t\t\t\t<img decoding=\"async\" width=\"591\" height=\"579\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2022\/06\/NANOVEA-Tribometer-T2000.png\" class=\"elementor-animation-grow attachment-medium_large size-medium_large wp-image-20089\" alt=\"Pneumatyczny trybometr NANOVEA T2000 do du\u017cych obci\u0105\u017ce\u0144\" \/>\t\t\t\t\t\t\t\t<\/a>\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-e767880 elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"e767880\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-no\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-da0379b\" data-id=\"da0379b\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-b8511cd elementor-widget elementor-widget-heading\" data-id=\"b8511cd\" data-element_type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\">PROCEDURY BADAWCZE<\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-3c63d98 elementor-widget elementor-widget-text-editor\" data-id=\"3c63d98\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p>Wsp\u00f3\u0142czynnik tarcia (COF) i skuteczno\u015b\u0107 \u015bcierania dw\u00f3ch rodzaj\u00f3w papier\u00f3w \u015bciernych oceniano za pomoc\u0105 trybometru NANOVEA T100. Jako materia\u0142 licznika zastosowano kulk\u0119 ze stali nierdzewnej 440. \u015alady zu\u017cycia pi\u0142ki badano po ka\u017cdym te\u015bcie zu\u017cycia za pomoc\u0105 NANOVEA <a href=\"https:\/\/nanovea.com\/profilometers\/\">Bezkontaktowy profiler optyczny 3D<\/a> aby zapewni\u0107 dok\u0142adne pomiary utraty obj\u0119to\u015bci.<\/p><p>Nale\u017cy pami\u0119ta\u0107, \u017ce jako materia\u0142 odniesienia wybrano kul\u0119 ze stali nierdzewnej 440, aby stworzy\u0107 badanie por\u00f3wnawcze, ale mo\u017cna zast\u0105pi\u0107 dowolny materia\u0142 sta\u0142y, aby zasymulowa\u0107 inne warunki zastosowania.<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<section class=\"elementor-section elementor-inner-section elementor-element elementor-element-b45cc31 elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"b45cc31\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-no\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-inner-column elementor-element elementor-element-0b0b9cc\" data-id=\"0b0b9cc\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-2752b9e elementor-widget elementor-widget-image\" data-id=\"2752b9e\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img decoding=\"async\" width=\"892\" height=\"501\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2021\/10\/Sandpaper-Abrasion-Test-Parameters.jpg\" class=\"attachment-large size-large wp-image-16033\" alt=\"parametry testowania \u015bcieralno\u015bci papieru \u015bciernego\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-inner-column elementor-element elementor-element-dfbb12c elementor-hidden-mobile\" data-id=\"dfbb12c\" data-element_type=\"column\" data-settings=\"{&quot;background_background&quot;:&quot;classic&quot;}\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-aed1bc3 elementor-widget elementor-widget-image\" data-id=\"aed1bc3\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img loading=\"lazy\" decoding=\"async\" width=\"758\" height=\"513\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2021\/10\/Sandpaper-Abrasion-Weat-Test.jpg\" class=\"attachment-large size-large wp-image-16034\" alt=\"Testy trybologiczne papieru \u015bciernego\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-1979bac elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"1979bac\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-no\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-c969083\" data-id=\"c969083\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-9c67049 elementor-widget elementor-widget-heading\" data-id=\"9c67049\" data-element_type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\">WYNIKI TEST\u00d3W I DYSKUSJA<\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-4c14a59 elementor-widget elementor-widget-text-editor\" data-id=\"4c14a59\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p>RYSUNEK 1 przedstawia por\u00f3wnanie COF papieru \u015bciernego 1 i 2 w suchych i mokrych warunkach otoczenia. Papier \u015bcierny 1 w warunkach suchych wykazuje na pocz\u0105tku testu wsp\u00f3\u0142czynnik COF r\u00f3wny 0,4, kt\u00f3ry stopniowo maleje i stabilizuje si\u0119 na poziomie 0,3. W warunkach wilgotnych pr\u00f3bka ta wykazuje ni\u017cszy \u015bredni wsp\u00f3\u0142czynnik COF wynosz\u0105cy 0,27. Natomiast wyniki COF pr\u00f3bki 2 wykazuj\u0105 COF w warunkach suchych na poziomie 0,27 i COF w warunkach mokrych na poziomie ~ 0,37.\u00a0<\/p><p>Nale\u017cy zwr\u00f3ci\u0107 uwag\u0119, \u017ce oscylacje w danych dla wszystkich wykres\u00f3w COF by\u0142y spowodowane drganiami generowanymi przez ruch \u015blizgowy kulki wzgl\u0119dem szorstkich powierzchni papieru \u015bciernego.<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<section class=\"elementor-section elementor-inner-section elementor-element elementor-element-f6f1994 elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"f6f1994\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-inner-column elementor-element elementor-element-64b2fd4\" data-id=\"64b2fd4\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-7d4ccd8 elementor-widget elementor-widget-image\" data-id=\"7d4ccd8\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img loading=\"lazy\" decoding=\"async\" width=\"634\" height=\"508\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2021\/10\/Sandpaper-Abrasion-COF.jpg\" class=\"attachment-large size-large wp-image-16030\" alt=\"papier \u015bcierny cof\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-9be55a4 elementor-widget elementor-widget-text-editor\" data-id=\"9be55a4\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p style=\"text-align: center;\"><span class=\"fontstyle0\" style=\"color: #1b96cf;\">RYSUNEK 1: <\/span><span class=\"fontstyle0\" style=\"color: #1b96cf;\"><span style=\"color: #000000;\"><span class=\"fontstyle0\">Ewolucja COF podczas test\u00f3w zu\u017cycia.<\/span> <br \/><\/span><\/span><\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-99b5f0a elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"99b5f0a\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-936bcc6\" data-id=\"936bcc6\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-2571aa5 elementor-widget elementor-widget-text-editor\" data-id=\"2571aa5\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p>RYSUNEK 2 podsumowuje wyniki analizy blizn po zu\u017cyciu. Pomiaru blizn dokonano przy u\u017cyciu mikroskopu optycznego oraz bezkontaktowego profilera optycznego NANOVEA 3D. RYSUNEK 3 i RYSUNEK 4 por\u00f3wnuj\u0105 blizny po zu\u017cyciu kulek SS440 po testach zu\u017cycia na papierze \u015bciernym 1 i 2 (warunki mokre i suche). Jak pokazano na RYSUNKU 4, Profiler Optyczny NANOVEA precyzyjnie uchwyci\u0142 topografi\u0119 powierzchni czterech kulek i ich \u015blady zu\u017cycia, kt\u00f3re nast\u0119pnie zosta\u0142y przetworzone przez oprogramowanie NANOVEA Mountains Advanced Analysis w celu obliczenia utraty obj\u0119to\u015bci i szybko\u015bci zu\u017cycia. Na obrazie mikroskopowym i profilowym kulki mo\u017cna zaobserwowa\u0107, \u017ce kulka u\u017cyta do test\u00f3w z papierem \u015bciernym 1 (na sucho) wykazuje wi\u0119ksz\u0105 sp\u0142aszczon\u0105 blizn\u0119 po zu\u017cyciu w por\u00f3wnaniu do pozosta\u0142ych z utrat\u0105 obj\u0119to\u015bci 0,313\u00a0<span style=\"color: #202124; font-family: Roboto, arial, sans-serif; font-size: 16px; text-align: left;\">mm<\/span><sup style=\"color: #202124; font-family: Roboto, arial, sans-serif; text-align: left;\">3<\/sup>. Natomiast strata obj\u0119to\u015bci dla papieru \u015bciernego 1 (na mokro) wynosi\u0142a 0,131\u00a0<span style=\"color: #202124; font-family: Roboto, arial, sans-serif; font-size: 16px; text-align: left;\">mm<\/span><sup style=\"color: #202124; font-family: Roboto, arial, sans-serif; text-align: left;\">3<\/sup>. W przypadku papieru \u015bciernego nr 2 (suchego) utrata obj\u0119to\u015bci wynosi\u0142a 0,163\u00a0<span style=\"color: #202124; font-family: Roboto, arial, sans-serif; font-size: 16px; text-align: left;\">mm<\/span><sup style=\"color: #202124; font-family: Roboto, arial, sans-serif; text-align: left;\">3<\/sup>\u00a0a dla papieru \u015bciernego 2 (mokrego) utrata obj\u0119to\u015bci wzros\u0142a do 0,237\u00a0<span style=\"color: #202124; font-family: Roboto, arial, sans-serif; font-size: 16px; text-align: left;\">mm<\/span><sup style=\"color: #202124; font-family: Roboto, arial, sans-serif; text-align: left;\">3<\/sup>.<\/p><p>Ponadto mo\u017cna zauwa\u017cy\u0107, \u017ce COF odgrywa\u0142 wa\u017cn\u0105 rol\u0119 w wydajno\u015bci \u015bcierania papier\u00f3w \u015bciernych. Papier \u015bcierny 1 wykazywa\u0142 wy\u017cszy COF w stanie suchym, co prowadzi\u0142o do wy\u017cszego wsp\u00f3\u0142czynnika \u015bcieralno\u015bci dla kulki SS440 u\u017cytej w te\u015bcie. Z kolei wy\u017cszy wsp\u00f3\u0142czynnik COF papieru \u015bciernego 2 w stanie mokrym skutkowa\u0142 wy\u017cszym wsp\u00f3\u0142czynnikiem \u015bcieralno\u015bci. \u015alady zu\u017cycia papier\u00f3w \u015bciernych po pomiarach przedstawiono na RYS. 5.<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<section class=\"elementor-section elementor-inner-section elementor-element elementor-element-5243fdc elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"5243fdc\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-inner-column elementor-element elementor-element-7b65061\" data-id=\"7b65061\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-0834b45 elementor-widget elementor-widget-text-editor\" data-id=\"0834b45\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p>Oba papiery \u015bcierne 1 i 2 twierdz\u0105, \u017ce dzia\u0142aj\u0105 zar\u00f3wno w suchym, jak i mokrym \u015brodowisku. Wykazywa\u0142y jednak znacz\u0105co r\u00f3\u017cn\u0105 skuteczno\u015b\u0107 \u015bcierania w warunkach suchych i mokrych. NANOVEA <a href=\"https:\/\/nanovea.com\/tribometers\/\">trybometry <\/a>zapewniaj\u0105 dobrze kontrolowane, wymierne i niezawodne mo\u017cliwo\u015bci oceny zu\u017cycia, kt\u00f3re zapewniaj\u0105 powtarzalne oceny zu\u017cycia. Co wi\u0119cej, mo\u017cliwo\u015b\u0107 pomiaru COF in situ pozwala u\u017cytkownikom powi\u0105za\u0107 r\u00f3\u017cne etapy procesu zu\u017cycia z ewolucj\u0105 COF, co ma kluczowe znaczenie dla poprawy podstawowego zrozumienia mechanizmu zu\u017cycia i w\u0142a\u015bciwo\u015bci tribologicznych papieru \u015bciernego<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-inner-column elementor-element elementor-element-2c86b20\" data-id=\"2c86b20\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-b124e96 elementor-widget elementor-widget-image\" data-id=\"b124e96\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img loading=\"lazy\" decoding=\"async\" width=\"507\" height=\"348\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2021\/10\/Sandpaper-Abrasion-Tribometer.jpg\" class=\"attachment-large size-large wp-image-16029\" alt=\"Testy trybologiczne \u015bcieralno\u015bci papieru \u015bciernego\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-1cb2f3a elementor-widget elementor-widget-text-editor\" data-id=\"1cb2f3a\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p style=\"text-align: center;\"><span class=\"fontstyle0\" style=\"color: #1b96cf;\">RYSUNEK 2: <\/span><span class=\"fontstyle0\" style=\"color: #1b96cf;\"><span style=\"color: #000000;\"><span class=\"fontstyle0\">Obj\u0119to\u015b\u0107 blizny po zu\u017cyciu kulek i \u015bredni COF w r\u00f3\u017cnych warunkach.<\/span><br \/><\/span><\/span><\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-fa6741e elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"fa6741e\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-9b17f53\" data-id=\"9b17f53\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<section class=\"elementor-section elementor-inner-section elementor-element elementor-element-12f15ce elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"12f15ce\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-inner-column elementor-element elementor-element-9bfb322\" data-id=\"9bfb322\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-6579947 elementor-widget elementor-widget-image\" data-id=\"6579947\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img loading=\"lazy\" decoding=\"async\" width=\"473\" height=\"439\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2021\/10\/Sandpaper-Abrasion-Dry-Wear-Test-1.jpg\" class=\"attachment-large size-large wp-image-16031\" alt=\"Test \u015bcieralno\u015bci papierem \u015bciernym - na sucho\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-inner-column elementor-element elementor-element-d116436\" data-id=\"d116436\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-32121fc elementor-widget elementor-widget-image\" data-id=\"32121fc\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img loading=\"lazy\" decoding=\"async\" width=\"474\" height=\"439\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2021\/10\/Sandpaper-Abrasion-Dry-Wear-Test-2.jpg\" class=\"attachment-large size-large wp-image-16032\" alt=\"Test \u015bcieralno\u015bci papieru \u015bciernego - na sucho\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-inner-section elementor-element elementor-element-5949d99 elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"5949d99\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-inner-column elementor-element elementor-element-95d1eab\" data-id=\"95d1eab\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-924abcb elementor-widget elementor-widget-image\" data-id=\"924abcb\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img loading=\"lazy\" decoding=\"async\" width=\"473\" height=\"440\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2021\/10\/Sandpaper-Abrasion-Wet-Wear-Test-1.jpg\" class=\"attachment-large size-large wp-image-16035\" alt=\"Test \u015bcieralno\u015bci papierem \u015bciernym - na mokro\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-inner-column elementor-element elementor-element-0b47d21\" data-id=\"0b47d21\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-a34cfe7 elementor-widget elementor-widget-image\" data-id=\"a34cfe7\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img loading=\"lazy\" decoding=\"async\" width=\"474\" height=\"440\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2021\/10\/Sandpaper-Abrasion-Wet-Wear-Test-2.jpg\" class=\"attachment-large size-large wp-image-16036\" alt=\"Test \u015bcieralno\u015bci papieru \u015bciernego - na mokro\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<div class=\"elementor-element elementor-element-60a7a04 elementor-widget elementor-widget-text-editor\" data-id=\"60a7a04\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p style=\"text-align: center;\"><span class=\"fontstyle0\" style=\"color: #1b96cf;\">RYSUNEK 3: <\/span><span class=\"fontstyle0\" style=\"color: #1b96cf;\"><span style=\"color: #000000;\"><span class=\"fontstyle0\">Blizny po noszeniu pi\u0142ek po testach.<\/span><br \/><\/span><\/span><\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-c34553d elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"c34553d\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-7cf53e9\" data-id=\"7cf53e9\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<section class=\"elementor-section elementor-inner-section elementor-element elementor-element-6de26da elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"6de26da\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-inner-column elementor-element elementor-element-1fbbe81\" data-id=\"1fbbe81\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-ab1e89b elementor-widget elementor-widget-image\" data-id=\"ab1e89b\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img loading=\"lazy\" decoding=\"async\" width=\"615\" height=\"445\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2021\/10\/Sandpaper-Dry-Profilometer-1.jpg\" class=\"attachment-large size-large wp-image-16037\" alt=\"\u015bcieranie papierem \u015bciernym - profilometria\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-inner-column elementor-element elementor-element-7bc2599\" data-id=\"7bc2599\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-4e44f33 elementor-widget elementor-widget-image\" data-id=\"4e44f33\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img loading=\"lazy\" decoding=\"async\" width=\"615\" height=\"445\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2021\/10\/Sandpaper-Dry-Profilometer-2.jpg\" class=\"attachment-large size-large wp-image-16038\" alt=\"\u015acieranie papierem \u015bciernym - profil powierzchni\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-inner-section elementor-element elementor-element-cd6b5bf elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"cd6b5bf\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-inner-column elementor-element elementor-element-f12cb8e\" data-id=\"f12cb8e\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-7d7f928 elementor-widget elementor-widget-image\" data-id=\"7d7f928\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img loading=\"lazy\" decoding=\"async\" width=\"615\" height=\"445\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2021\/10\/Sandpaper-Wet-Profilometer-1.jpg\" class=\"attachment-large size-large wp-image-16043\" alt=\"Test \u015bcieralno\u015bci papierem \u015bciernym - profil powierzchni 3d\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-inner-column elementor-element elementor-element-9de0742\" data-id=\"9de0742\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-0f391dd elementor-widget elementor-widget-image\" data-id=\"0f391dd\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img loading=\"lazy\" decoding=\"async\" width=\"615\" height=\"445\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2021\/10\/Sandpaper-Wet-Profilometer-2.jpg\" class=\"attachment-large size-large wp-image-16044\" alt=\"Test \u015bcieralno\u015bci papieru \u015bciernego - skanowanie powierzchni 3d\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<div class=\"elementor-element elementor-element-dabaf49 elementor-widget elementor-widget-text-editor\" data-id=\"dabaf49\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p style=\"text-align: center;\"><span class=\"fontstyle0\" style=\"color: #1b96cf;\">RYSUNEK 4: <\/span><span class=\"fontstyle0\" style=\"color: #1b96cf;\"><span style=\"color: #000000;\"><span class=\"fontstyle0\">Morfologia 3D blizn zu\u017cycia na kulkach.<\/span><br \/><\/span><\/span><\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-d910ad4 elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"d910ad4\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-f639602\" data-id=\"f639602\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<section class=\"elementor-section elementor-inner-section elementor-element elementor-element-45d22ed elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"45d22ed\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-inner-column elementor-element elementor-element-55650fc\" data-id=\"55650fc\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-e1b6f1e elementor-widget elementor-widget-image\" data-id=\"e1b6f1e\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img loading=\"lazy\" decoding=\"async\" width=\"512\" height=\"469\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2021\/10\/Sandpaper-Wear-Test-Dry-1.jpg\" class=\"attachment-large size-large wp-image-16039\" alt=\"Wyniki testu \u015bcieralno\u015bci papieru \u015bciernego\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-inner-column elementor-element elementor-element-74b8658\" data-id=\"74b8658\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-06caf52 elementor-widget elementor-widget-image\" data-id=\"06caf52\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img loading=\"lazy\" decoding=\"async\" width=\"511\" height=\"469\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2021\/10\/Sandpaper-Wear-Test-Dry-2.jpg\" class=\"attachment-large size-large wp-image-16040\" alt=\"Wyniki test\u00f3w \u015bcieralno\u015bci papieru \u015bciernego\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-inner-section elementor-element elementor-element-08577af elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"08577af\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-inner-column elementor-element elementor-element-566bb8b\" data-id=\"566bb8b\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-19f02a8 elementor-widget elementor-widget-image\" data-id=\"19f02a8\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img loading=\"lazy\" decoding=\"async\" width=\"512\" height=\"469\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2021\/10\/Sandpaper-Wear-Test-Wet-1.jpg\" class=\"attachment-large size-large wp-image-16041\" alt=\"Wyniki testu trybologicznego \u015bcieralno\u015bci papieru \u015bciernego\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-inner-column elementor-element elementor-element-507e7a3\" data-id=\"507e7a3\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-b0dbabf elementor-widget elementor-widget-image\" data-id=\"b0dbabf\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img loading=\"lazy\" decoding=\"async\" width=\"511\" height=\"468\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2021\/10\/Sandpaper-Wear-Test-Wet-2.jpg\" class=\"attachment-large size-large wp-image-16042\" alt=\"Wyniki test\u00f3w \u015bcieralno\u015bci papieru \u015bciernego\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<div class=\"elementor-element elementor-element-db6c287 elementor-widget elementor-widget-text-editor\" data-id=\"db6c287\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p style=\"text-align: center;\"><span class=\"fontstyle0\" style=\"color: #1b96cf;\">RYSUNEK 5: <\/span><span class=\"fontstyle0\" style=\"color: #1b96cf;\"><span style=\"color: #000000;\"><span class=\"fontstyle0\">\u015alady zu\u017cycia na papierach \u015bciernych w r\u00f3\u017cnych warunkach.<\/span><br \/><\/span><\/span><\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-9c9a5b1 elementor-section-content-middle elementor-reverse-mobile elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"9c9a5b1\" data-element_type=\"section\" data-settings=\"{&quot;background_background&quot;:&quot;classic&quot;}\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-top-column elementor-element elementor-element-f2d1204 elementor-hidden-phone\" data-id=\"f2d1204\" data-element_type=\"column\" data-settings=\"{&quot;background_background&quot;:&quot;classic&quot;}\">\n\t\t\t<div class=\"elementor-widget-wrap\">\n\t\t\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-top-column elementor-element elementor-element-3f87574\" data-id=\"3f87574\" data-element_type=\"column\" data-settings=\"{&quot;background_background&quot;:&quot;classic&quot;}\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-8843a9f elementor-widget elementor-widget-heading\" data-id=\"8843a9f\" data-element_type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\">PODSUMOWANIE<\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-18f7f2e elementor-widget elementor-widget-text-editor\" data-id=\"18f7f2e\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p>W niniejszej pracy oceniono wydajno\u015b\u0107 \u015bcierania dw\u00f3ch rodzaj\u00f3w papier\u00f3w \u015bciernych o tej samej liczbie ziarna w warunkach suchych i mokrych. Warunki u\u017cytkowania papieru \u015bciernego odgrywaj\u0105 decyduj\u0105c\u0105 rol\u0119 w efektywno\u015bci pracy. Papier \u015bcierny nr 1 wykazywa\u0142 wyra\u017anie lepsze w\u0142a\u015bciwo\u015bci \u015bcierne w warunkach suchych, natomiast papier \u015bcierny nr 2 lepiej zachowywa\u0142 si\u0119 w warunkach mokrych. Tarcie podczas procesu szlifowania jest wa\u017cnym czynnikiem, kt\u00f3ry nale\u017cy wzi\u0105\u0107 pod uwag\u0119 przy ocenie wydajno\u015bci \u015bcierania. Profiler optyczny NANOVEA precyzyjnie mierzy morfologi\u0119 3D ka\u017cdej powierzchni, np. blizny po zu\u017cyciu na pi\u0142ce, co zapewnia wiarygodn\u0105 ocen\u0119 wydajno\u015bci \u015bcierania papieru \u015bciernego w tym badaniu. Tribometr NANOVEA mierzy wsp\u00f3\u0142czynnik tarcia in situ podczas testu zu\u017cycia, zapewniaj\u0105c wgl\u0105d w r\u00f3\u017cne etapy procesu zu\u017cycia. Oferuje powtarzalne badania zu\u017cycia i tarcia w trybach obrotowym i liniowym zgodnych z normami ISO i ASTM, z opcjonalnymi modu\u0142ami do bada\u0144 zu\u017cycia w wysokiej temperaturze i smarowania dost\u0119pnymi w jednym, wst\u0119pnie zintegrowanym systemie. Ten niezr\u00f3wnany zakres pozwala u\u017cytkownikom symulowa\u0107 r\u00f3\u017cne ci\u0119\u017ckie \u015brodowiska pracy \u0142o\u017cysk kulkowych, w tym wysokie napr\u0119\u017cenia, zu\u017cycie i wysok\u0105 temperatur\u0119, itp. Stanowi on r\u00f3wnie\u017c idealne narz\u0119dzie do ilo\u015bciowej oceny zachowa\u0144 trybologicznych materia\u0142\u00f3w o najwy\u017cszej odporno\u015bci na zu\u017cycie pod du\u017cymi obci\u0105\u017ceniami.<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-f8f5f67 elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"f8f5f67\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-a8891e3\" data-id=\"a8891e3\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-0ef778b elementor-widget elementor-widget-heading\" data-id=\"0ef778b\" data-element_type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\">Masz podobn\u0105 aplikacj\u0119?<\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-07a7a14 elementor-align-justify open-chat elementor-widget elementor-widget-button\" data-id=\"07a7a14\" data-element_type=\"widget\" data-widget_type=\"button.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<div class=\"elementor-button-wrapper\">\n\t\t\t\t\t<a class=\"elementor-button elementor-size-sm\" role=\"button\">\n\t\t\t\t\t\t<span class=\"elementor-button-content-wrapper\">\n\t\t\t\t\t\t\t\t\t<span class=\"elementor-button-text\">POROZMAWIAJ Z EKSPERTEM JU\u017b TERAZ<\/span>\n\t\t\t\t\t<\/span>\n\t\t\t\t\t<\/a>\n\t\t\t\t<\/div>\n\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-5818d0a elementor-align-justify button-quote elementor-widget elementor-widget-button\" data-id=\"5818d0a\" data-element_type=\"widget\" data-widget_type=\"button.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<div class=\"elementor-button-wrapper\">\n\t\t\t\t\t<a class=\"elementor-button elementor-button-link elementor-size-sm\" href=\"https:\/\/nanovea.com\/contact-sales-form\/\" id=\"button-quote-bottom\">\n\t\t\t\t\t\t<span class=\"elementor-button-content-wrapper\">\n\t\t\t\t\t\t\t\t\t<span class=\"elementor-button-text\">SZYBKA WYCENA I SZCZEG\u00d3\u0141OWE INFORMACJE<\/span>\n\t\t\t\t\t<\/span>\n\t\t\t\t\t<\/a>\n\t\t\t\t<\/div>\n\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<\/div>","protected":false},"excerpt":{"rendered":"<p>SANDPAPER ABRASION PERFORMANCE USING A TRIBOMETER Prepared by DUANJIE LI, PhD INTRODUCTION Sandpaper consists of abrasive particles glued to one face of a paper or cloth. Various abrasive materials can be used for the particles, such as garnet, silicon carbide, aluminum oxide and diamond. Sandpaper is widely applied in a variety of industrial sectors to [&hellip;]<\/p>\n","protected":false},"author":1,"featured_media":16073,"comment_status":"open","ping_status":"open","sticky":false,"template":"","format":"standard","meta":{"_exactmetrics_skip_tracking":false,"_exactmetrics_sitenote_active":false,"_exactmetrics_sitenote_note":"","_exactmetrics_sitenote_category":0,"footnotes":""},"categories":[7,349,380,355,335,373,336],"tags":[],"class_list":["post-16045","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-application-notes","category-laboratory-testing","category-liquid-tribology","category-profilometry-volume-area","category-profilometry-testing","category-rotational-tribology","category-tribology-testing"],"_links":{"self":[{"href":"https:\/\/nanovea.com\/pl\/wp-json\/wp\/v2\/posts\/16045","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/nanovea.com\/pl\/wp-json\/wp\/v2\/posts"}],"about":[{"href":"https:\/\/nanovea.com\/pl\/wp-json\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"https:\/\/nanovea.com\/pl\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/nanovea.com\/pl\/wp-json\/wp\/v2\/comments?post=16045"}],"version-history":[{"count":66,"href":"https:\/\/nanovea.com\/pl\/wp-json\/wp\/v2\/posts\/16045\/revisions"}],"predecessor-version":[{"id":24581,"href":"https:\/\/nanovea.com\/pl\/wp-json\/wp\/v2\/posts\/16045\/revisions\/24581"}],"wp:featuredmedia":[{"embeddable":true,"href":"https:\/\/nanovea.com\/pl\/wp-json\/wp\/v2\/media\/16073"}],"wp:attachment":[{"href":"https:\/\/nanovea.com\/pl\/wp-json\/wp\/v2\/media?parent=16045"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"https:\/\/nanovea.com\/pl\/wp-json\/wp\/v2\/categories?post=16045"},{"taxonomy":"post_tag","embeddable":true,"href":"https:\/\/nanovea.com\/pl\/wp-json\/wp\/v2\/tags?post=16045"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}