{"id":8344,"date":"2020-05-11T05:07:45","date_gmt":"2020-05-11T05:07:45","guid":{"rendered":"https:\/\/nanovea.com\/?p=8344"},"modified":"2023-11-13T22:17:52","modified_gmt":"2023-11-13T22:17:52","slug":"%eb%b8%94%eb%a1%9d-%ec%98%a8-%eb%a7%81-%ec%8a%ac%eb%9d%bc%ec%9d%b4%eb%94%a9-%eb%a7%88%eb%aa%a8-%ed%8f%89%ea%b0%80","status":"publish","type":"post","link":"https:\/\/nanovea.com\/ko\/block-on-ring-sliding-wear-evaluation\/","title":{"rendered":"\ube14\ub85d-\uc628-\ub9c1 \ub9c8\ubaa8 \ud14c\uc2a4\ud2b8"},"content":{"rendered":"<div data-elementor-type=\"wp-post\" data-elementor-id=\"8344\" class=\"elementor elementor-8344\" data-elementor-post-type=\"post\">\n\t\t\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-3a9803e6 elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"3a9803e6\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-13caf891\" data-id=\"13caf891\" data-element_type=\"column\" data-settings=\"{&quot;background_background&quot;:&quot;classic&quot;}\">\n\t\t\t<div class=\"elementor-widget-wrap\">\n\t\t\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-1a5e82a6 elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"1a5e82a6\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-77960ac2\" data-id=\"77960ac2\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-634241d9 elementor-widget elementor-widget-text-editor\" data-id=\"634241d9\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p style=\"text-align: left; color: #1b96cf; font-size: 24px; line-height: 30px;\"><strong><em>\ube14\ub85d \uc628 \ub9c1 \ub9c8\ubaa8 \ud3c9\uac00\uc758 \uc911\uc694\uc131<\/em><u><i><br \/><\/i><\/u><\/strong><\/p><div>\uc2ac\ub77c\uc774\ub529 \ub9c8\ubaa8\ub294 \ud558\uc911\uc744 \ubc1b\ub294 \uc811\ucd09 \ubd80\uc704\uc5d0\uc11c \ub450 \uc18c\uc7ac\uac00 \uc11c\ub85c \ubbf8\ub044\ub7ec\uc9c0\uba74\uc11c \ubc1c\uc0dd\ud558\ub294 \uc810\uc9c4\uc801\uc778 \uc18c\uc7ac \uc190\uc2e4\uc785\ub2c8\ub2e4. \uc2ac\ub77c\uc774\ub529 \ub9c8\ubaa8\ub294 \uc790\ub3d9\ucc28, \ud56d\uacf5\uc6b0\uc8fc, \uc11d\uc720 \ubc0f \uac00\uc2a4 \ub4f1 \uae30\uacc4\uc640 \uc5d4\uc9c4\uc774 \uc791\ub3d9\ud558\ub294 \ub2e4\uc591\ud55c \uc0b0\uc5c5\uc5d0\uc11c \ud544\uc5f0\uc801\uc73c\ub85c \ubc1c\uc0dd\ud569\ub2c8\ub2e4. \uc774\ub7ec\ud55c \uc2ac\ub77c\uc774\ub529 \ub3d9\uc791\uc740 \ud45c\uba74\uc5d0\uc11c \uc2ec\uac01\ud55c \uae30\uacc4\uc801 \ub9c8\ubaa8\uc640 \uc7ac\ub8cc \uc774\ub3d9\uc744 \uc720\ubc1c\ud558\uc5ec \uc0dd\uc0b0 \ud6a8\uc728\uc131, \uae30\uacc4 \uc131\ub2a5\uc744 \uc800\ud558\uc2dc\ud0a4\uac70\ub098 \uc2ec\uc9c0\uc5b4 \uae30\uacc4\uc5d0 \uc190\uc0c1\uc744 \uc785\ud790 \uc218 \uc788\uc2b5\ub2c8\ub2e4.<\/div><div>\u00a0<\/div><p>\u00a0<\/p><div>\uc2ac\ub77c\uc774\ub529 \ub9c8\ubaa8\uc5d0\ub294 \uc811\ucc29 \ub9c8\ubaa8, 2\uccb4 \ub9c8\ubaa8, 3\uccb4 \ub9c8\ubaa8 \ubc0f \ud53c\ub85c \ub9c8\ubaa8\uc640 \uac19\uc740 \uc811\ucd09 \ud45c\uba74\uc5d0\uc11c \ubc1c\uc0dd\ud558\ub294 \ubcf5\uc7a1\ud55c \ub9c8\ubaa8 \uba54\ucee4\ub2c8\uc998\uc774 \ud3ec\ud568\ub418\ub294 \uacbd\uc6b0\uac00 \ub9ce\uc2b5\ub2c8\ub2e4. \uc7ac\ub8cc\uc758 \ub9c8\ubaa8 \uac70\ub3d9\uc740 \uc815\uc0c1 \ud558\uc911, \uc18d\ub3c4, \ubd80\uc2dd \ubc0f \uc724\ud65c\uacfc \uac19\uc740 \uc791\uc5c5 \ud658\uacbd\uc5d0 \uc758\ud574 \ud06c\uac8c \uc601\ud5a5\uc744 \ubc1b\uc2b5\ub2c8\ub2e4. \ub2e4\uc7ac\ub2e4\ub2a5\ud55c <a href=\"https:\/\/nanovea.com\/tribometers\/\">\ud2b8\ub77c\uc774\ubcf4\ubbf8\ud130 <\/a>\ub2e4\uc591\ud55c \uc2e4\uc81c \uc791\uc5c5 \uc870\uac74\uc744 \uc2dc\ubbac\ub808\uc774\uc158\ud560 \uc218 \uc788\ub294 \uac83\uc774 \ub9c8\ubaa8 \ud3c9\uac00\uc5d0 \uc774\uc0c1\uc801\uc785\ub2c8\ub2e4.<br \/>Block-on-Ring(ASTM G77) \ud14c\uc2a4\ud2b8\ub294 \ub2e4\uc591\ud55c \uc2dc\ubbac\ub808\uc774\uc158 \uc870\uac74\uc5d0\uc11c \uc7ac\ub8cc\uc758 \uc2ac\ub77c\uc774\ub529 \ub9c8\ubaa8 \uac70\ub3d9\uc744 \ud3c9\uac00\ud558\ub294 \ub110\ub9ac \uc0ac\uc6a9\ub418\ub294 \uae30\uc220\ub85c, \ud2b9\uc815 \ub9c8\ucc30 \uacf5\ud559 \uc751\uc6a9 \ubd84\uc57c\uc5d0 \ub300\ud574 \uc2e0\ub8b0\ud560 \uc218 \uc788\ub294 \uc7ac\ub8cc \ucee4\ud50c \uc21c\uc704\ub97c \uc9c0\uc815\ud560 \uc218 \uc788\uc2b5\ub2c8\ub2e4.<\/div><div>\u00a0<\/div><div>\u00a0<\/div><p>\u00a0<\/p><p style=\"text-align: left; color: #1b96cf; font-size: 24px; line-height: 30px;\"><strong><em>\uce21\uc815 \ubaa9\ud45c<\/em><u><i><br \/><\/i><\/u><\/strong><\/p><p>\uc774 \uc751\uc6a9 \ubd84\uc57c\uc5d0\uc11c \ub098\ub178\ubca0\uc544 \uae30\uacc4\uc2dd \ud14c\uc2a4\ud130\ub294 \uc2a4\ud14c\uc778\ub9ac\uc2a4 \uc2a4\ud2f8 SS304 \ubc0f \uc54c\ub8e8\ubbf8\ub284 Al6061 \uae08\uc18d \ud569\uae08 \uc2dc\ub8cc\uc758 YS \ubc0f UTS\ub97c \uce21\uc815\ud569\ub2c8\ub2e4. \uc0d8\ud50c\uc740 \ub098\ub178\ubca0\uc544 \uc555\uc785 \ubc29\ubc95\uc758 \uc2e0\ub8b0\uc131\uc744 \ubcf4\uc5ec\uc8fc\ub294 \uc77c\ubc18\uc801\uc73c\ub85c \uc778\uc815\ub418\ub294 YS \ubc0f UTS \uac12\uc744 \uc704\ud574 \uc120\ud0dd\ub418\uc5c8\uc2b5\ub2c8\ub2e4.<\/p><p>\u00a0<\/p><div style=\"text-align: center;\"><a href=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/05\/Figure-1.png\"><img fetchpriority=\"high\" decoding=\"async\" class=\"alignnone size-full wp-image-8348\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/05\/Figure-1.png\" alt=\"\" width=\"648\" height=\"408\" \/><\/a><\/div><p>S-10 \ub9c1\uc5d0 \uc788\ub294 H-30 \ube14\ub85d\uc758 \uc2ac\ub77c\uc774\ub529 \ub9c8\ubaa8 \uac70\ub3d9\uc740 Block-on-Ring \ubaa8\ub4c8\uc744 \uc0ac\uc6a9\ud558\ub294 Nanovea \ub9c8\ucc30\uacc4\ub85c \ud3c9\uac00\ub418\uc5c8\uc2b5\ub2c8\ub2e4. H-30 \ube14\ub85d\uc740 \uacbd\ub3c4\uac00 30HRC\uc778 01 \uacf5\uad6c\uac15\uc73c\ub85c \uc81c\uc791\ub418\ub294 \ubc18\uba74, S-10 \ub9c1\uc740 \ud45c\uba74 \uacbd\ub3c4\uac00 58~63HRC\uc774\uace0 \ub9c1 \uc9c1\uacbd\uc774 ~34.98mm\uc778 \uac15\ucca0 \uc720\ud615 4620\uc785\ub2c8\ub2e4. Block-on-Ring \ud14c\uc2a4\ud2b8\ub294 \ub9c8\ubaa8 \uac70\ub3d9\uc5d0 \ub300\ud55c \uc601\ud5a5\uc744 \uc870\uc0ac\ud558\uae30 \uc704\ud574 \uac74\uc870\ud558\uace0 \uc724\ud65c\ub41c \ud658\uacbd\uc5d0\uc11c \uc218\ud589\ub418\uc5c8\uc2b5\ub2c8\ub2e4. USP \uc911\uc9c8 \ubbf8\ub124\ub784 \uc624\uc77c\uc744 \uc0ac\uc6a9\ud558\uc5ec \uc724\ud65c \ud14c\uc2a4\ud2b8\ub97c \uc218\ud589\ud588\uc2b5\ub2c8\ub2e4. \ub9c8\ubaa8 \ud2b8\ub799\uc740 Nanovea\ub97c \uc0ac\uc6a9\ud558\uc5ec \uac80\uc0ac\ub418\uc5c8\uc2b5\ub2c8\ub2e4. <a href=\"https:\/\/nanovea.com\/profilometers\/\">3D \ube44\uc811\ucd09 \ud504\ub85c\ud30c\uc77c\ub85c\ubbf8\ud130<\/a>. \uc2dc\ud5d8 \ubcc0\uc218\ub294 \ud45c 1\uc5d0 \uc694\uc57d\ub418\uc5b4 \uc788\uc2b5\ub2c8\ub2e4. \ub9c8\ubaa8\uc728(K)\uc740 K=V\/(F\u00d7s) \uacf5\uc2dd\uc744 \uc0ac\uc6a9\ud558\uc5ec \ud3c9\uac00\ub418\uc5c8\uc73c\uba70, \uc5ec\uae30\uc11c V\ub294 \ub9c8\ubaa8\ub7c9, F\ub294 \uc77c\ubc18 \ud558\uc911, s\ub294 \uc2ac\ub77c\uc774\ub529 \uac70\ub9ac\uc785\ub2c8\ub2e4.<\/p><p>\u00a0<\/p><div style=\"text-align: center;\"><a href=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/05\/Table-1.png\"><img decoding=\"async\" class=\"alignnone size-full wp-image-8349\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/05\/Table-1.png\" alt=\"\" width=\"450\" height=\"106\" \/><\/a><\/div><p>\u00a0<\/p><p style=\"text-align: left; color: #1b96cf; font-size: 24px; line-height: 30px;\"><strong><em>\uacb0\uacfc \ubc0f \ud1a0\ub860<\/em><u><i><br \/><\/i><\/u><\/strong><\/p><p style=\"margin: 0in; margin-bottom: .0001pt;\"><span style=\"font-family: 'Arial',sans-serif;\">\uadf8\ub9bc 2\ub294 \uac74\uc870\ud558\uace0 \uc724\ud65c\ub41c \ud658\uacbd\uc5d0\uc11c Block-on-Ring \ud14c\uc2a4\ud2b8\uc758 \ub9c8\ucc30 \uacc4\uc218(COF)\ub97c \ube44\uad50\ud569\ub2c8\ub2e4. \ube14\ub85d\uc740 \uc724\ud65c \ud658\uacbd\ubcf4\ub2e4 \uac74\uc870\ud55c \ud658\uacbd\uc5d0\uc11c \ud6e8\uc52c \ub354 \ub9ce\uc740 \ub9c8\ucc30\uc744 \uac16\uc2b5\ub2c8\ub2e4. COF<br \/>\uccab \ubc88\uc9f8 50\ud68c\uc804\uc5d0\uc11c \ub7f0\uc778 \uae30\uac04 \ub3d9\uc548 \ubcc0\ub3d9\ud558\uace0 \ub098\uba38\uc9c0 200\ud68c\uc804 \ub9c8\ubaa8 \ud14c\uc2a4\ud2b8\uc5d0\uc11c\ub294 ~0.8\uc758 \uc77c\uc815\ud55c COF\uc5d0 \ub3c4\ub2ec\ud569\ub2c8\ub2e4. \uc774\uc5d0 \ube44\ud574 USP \uc911\uc9c8\uad11\uc720 \uc724\ud65c\uc5d0\uc11c \uc218\ud589\ub41c Block-on-Ring \ud14c\uc2a4\ud2b8\ub294 500,000\ud68c\uc804 \ub9c8\ubaa8 \ud14c\uc2a4\ud2b8 \uc804\uccb4\uc5d0\uc11c 0.09\uc758 \uc77c\uc815\ud558\uace0 \ub0ae\uc740 COF\ub97c \ub098\ud0c0\ub0c5\ub2c8\ub2e4. \uc724\ud65c\uc81c\ub294 \ud45c\uba74 \uc0ac\uc774\uc758 COF\ub97c ~90\ubc30\uae4c\uc9c0 \ud06c\uac8c \uc904\uc785\ub2c8\ub2e4.<\/span><\/p><p style=\"margin: 0in; margin-bottom: .0001pt;\">\u00a0<\/p><p>\uadf8\ub9bc 3\uacfc 4\ub294 \uac74\uc2dd \ubc0f \uc724\ud65c \ub9c8\ubaa8 \ud14c\uc2a4\ud2b8 \ud6c4 \ube14\ub85d\uc758 \ub9c8\ubaa8 \ud749\ud130\uc5d0 \ub300\ud55c \uad11\ud559 \uc774\ubbf8\uc9c0\uc640 \ub2e8\uba74 2D \ud504\ub85c\ud30c\uc77c\uc744 \ubcf4\uc5ec\uc90d\ub2c8\ub2e4. \ub9c8\ubaa8 \ud2b8\ub799 \ubd80\ud53c\uc640 \ub9c8\ubaa8\uc728\uc740 \ud45c 2\uc5d0 \ub098\uc640 \uc788\uc2b5\ub2c8\ub2e4. 200\ud68c\uc804 \ub3d9\uc548 72rpm\uc758 \ub0ae\uc740 \ud68c\uc804 \uc18d\ub3c4\uc5d0\uc11c \uac74\uc2dd \ub9c8\ubaa8 \ud14c\uc2a4\ud2b8\ub97c \uac70\uce5c \uc2a4\ud2f8 \ube14\ub85d\uc740 9.45mm\u02d9\uc758 \ud070 \ub9c8\ubaa8 \ud749\ud130 \ubd80\ud53c\ub97c \ub098\ud0c0\ub0c5\ub2c8\ub2e4. \uc774\uc5d0 \ube44\ud574 \uad11\uc720 \uc724\ud65c\uc720\ub97c \uc0ac\uc6a9\ud558\uc5ec 500,000\ud68c\uc804 \ub3d9\uc548 197rpm\uc758 \ub192\uc740 \ud68c\uc804 \uc18d\ub3c4\ub85c \ub9c8\ubaa8 \ud14c\uc2a4\ud2b8\ub97c \uc218\ud589\ud55c \uacbd\uc6b0 \ub9c8\ubaa8 \ud2b8\ub799 \ubd80\ud53c\ub294 0.03mm\u02d9\ub85c \ud6e8\uc52c \uc791\uc544\uc9d1\ub2c8\ub2e4.<\/p><p>\u00a0<\/p><p style=\"margin: 0in; margin-bottom: .0001pt;\"><span style=\"font-family: 'Arial',sans-serif;\"><br \/>\uadf8\ub9bc 3\uc758 \uc774\ubbf8\uc9c0\ub294 \uc724\ud65c \ub9c8\ubaa8 \ud14c\uc2a4\ud2b8\uc758 \uacbd\ubbf8\ud55c \ub9c8\ubaa8\uc640 \ube44\uad50\ud558\uc5ec \uac74\uc870\ud55c \uc870\uac74\uc5d0\uc11c \ud14c\uc2a4\ud2b8\ud558\ub294 \ub3d9\uc548 \uc2ec\uac01\ud55c \ub9c8\ubaa8\uac00 \ubc1c\uc0dd\ud558\ub294 \uac83\uc744 \ubcf4\uc5ec\uc90d\ub2c8\ub2e4. \uac74\uc2dd \ub9c8\ubaa8 \ud14c\uc2a4\ud2b8 \uc911\uc5d0 \ubc1c\uc0dd\ud558\ub294 \ub192\uc740 \uc5f4\uacfc \uac15\ud55c \uc9c4\ub3d9\uc740 \uae08\uc18d \ud30c\ud3b8\uc758 \uc0b0\ud654\ub97c \ucd09\uc9c4\ud558\uc5ec \uc2ec\uac01\ud55c \uc0bc\uccb4 \ub9c8\ubaa8\ub97c \uc720\ubc1c\ud569\ub2c8\ub2e4. \uc724\ud65c \ud14c\uc2a4\ud2b8\uc5d0\uc11c\ub294 \ubbf8\ub124\ub784 \uc624\uc77c\uc774 \ub9c8\ucc30\uc744 \uc904\uc774\uace0 \uc811\ucd09\uba74\uc744 \ub0c9\uac01\uc2dc\ud0ac \ubfd0\ub9cc \uc544\ub2c8\ub77c \ub9c8\ubaa8 \uc911\uc5d0 \uc0dd\uc131\ub41c \uc5f0\ub9c8 \ud30c\ud3b8\uc744 \uba40\ub9ac \uc774\ub3d9\uc2dc\ud0b5\ub2c8\ub2e4. \uadf8 \uacb0\uacfc \ub9c8\ubaa8\uc728\uc774 \ucd5c\ub300 8\u00d710\ubc30\uae4c\uc9c0 \ud604\uc800\ud788 \uac10\uc18c\ud569\ub2c8\ub2e4. \uc774\ucc98\ub7fc \uc11c\ub85c \ub2e4\ub978 \ud658\uacbd\uc5d0\uc11c \ub0b4\ub9c8\ubaa8\uc131\uc5d0 \ud070 \ucc28\uc774\ub97c \ubcf4\uc774\ub294 \uac83\uc740 \uc2e4\uc81c \uc11c\ube44\uc2a4 \uc870\uac74\uc5d0\uc11c \uc801\uc808\ud55c \uc2ac\ub77c\uc774\ub529 \ub9c8\ubaa8 \uc2dc\ubbac\ub808\uc774\uc158\uc774 \uc911\uc694\ud558\ub2e4\ub294 \uac83\uc744 \ubcf4\uc5ec\uc90d\ub2c8\ub2e4.<\/span><\/p><p>\u00a0<\/p><p style=\"margin: 0in; margin-bottom: .0001pt;\"><span style=\"font-family: 'Arial',sans-serif;\"><br \/>\ud14c\uc2a4\ud2b8 \uc870\uac74\uc5d0 \uc791\uc740 \ubcc0\ud654\uac00 \uc0dd\uae30\uba74 \ub9c8\ubaa8 \uac70\ub3d9\uc774 \ud06c\uac8c \ub2ec\ub77c\uc9c8 \uc218 \uc788\uc2b5\ub2c8\ub2e4. \ub098\ub178\ubca0\uc544 \ud2b8\ub77c\uc774\ubcf4\ubbf8\ud130\uc758 \ub2e4\uc591\ud55c \uae30\ub2a5 \ub355\ubd84\uc5d0 \uace0\uc628, \uc724\ud65c \ubc0f \ub9c8\ucc30 \ubd80\uc2dd \uc870\uac74\uc5d0\uc11c \ub9c8\ubaa8\ub97c \uce21\uc815\ud560 \uc218 \uc788\uc2b5\ub2c8\ub2e4. \uace0\uae09 \ubaa8\ud130\uc5d0 \uc758\ud55c \uc815\ud655\ud55c \uc18d\ub3c4 \ubc0f \uc704\uce58 \uc81c\uc5b4\ub97c \ud1b5\ud574 0.001 ~ 5000rpm \ubc94\uc704\uc758 \uc18d\ub3c4\uc5d0\uc11c \ub9c8\ubaa8 \ud14c\uc2a4\ud2b8\ub97c \uc218\ud589\ud560 \uc218 \uc788\uc73c\ubbc0\ub85c \ub2e4\uc591\ud55c \ub9c8\ucc30 \uc870\uac74\uc5d0\uc11c \ub9c8\ubaa8\ub97c \uc870\uc0ac\ud558\ub294 \uc5f0\uad6c\/\ud14c\uc2a4\ud2b8 \uc2e4\ud5d8\uc2e4\uc5d0 \uc774\uc0c1\uc801\uc778 \ub3c4\uad6c\uc785\ub2c8\ub2e4.<\/span><\/p><p style=\"margin: 0in; margin-bottom: .0001pt;\">\u00a0<\/p><p>\uc0d8\ud50c\uc758 \ud45c\uba74 \uc0c1\ud0dc\ub294 \ub098\ub178\ube44\uc544\uc758 \ube44\uc811\ucd09\uc2dd \uad11\ud559 \ud504\ub85c\ub85c\ubbf8\ud130\ub85c \uac80\uc0ac\ud588\uc2b5\ub2c8\ub2e4. \uadf8\ub9bc 5\ub294 \ub9c8\ubaa8 \ud14c\uc2a4\ud2b8 \ud6c4 \ub9c1\uc758 \ud45c\uba74 \ud615\ud0dc\ub97c \ubcf4\uc5ec\uc90d\ub2c8\ub2e4. \uc2ac\ub77c\uc774\ub529 \ub9c8\ubaa8 \uacfc\uc815\uc5d0\uc11c \uc0dd\uc131\ub41c \ud45c\uba74 \ud615\ud0dc\uc640 \uac70\uce60\uae30\ub97c \ub354 \uc798 \ubcf4\uc5ec\uc8fc\uae30 \uc704\ud574 \uc2e4\ub9b0\ub354 \ud615\ud0dc\ub97c \uc81c\uac70\ud588\uc2b5\ub2c8\ub2e4. 200 \ud68c\uc804\uc758 \uac74\uc2dd \ub9c8\ubaa8 \ud14c\uc2a4\ud2b8 \ub3d9\uc548 3\uccb4 \ub9c8\ubaa8 \uacf5\uc815\uc73c\ub85c \uc778\ud574 \uc0c1\ub2f9\ud55c \ud45c\uba74 \uac70\uce60\uae30\uac00 \ubc1c\uc0dd\ud588\uc2b5\ub2c8\ub2e4. \uac74\uc2dd \ub9c8\ubaa8 \ud14c\uc2a4\ud2b8 \ud6c4 \ube14\ub85d\uacfc \ub9c1\uc740 \uac01\uac01 14.1 \ubc0f 18.1 \u00b5m\uc758 \uac70\uce60\uae30 Ra\ub97c \ubcf4\uc600\ub294\ub370, \uc774\ub294 \ub354 \ub192\uc740 \uc18d\ub3c4\uc5d0\uc11c \uc7a5\uae30\uac04 500,000\ud68c\uc804 \uc724\ud65c \ub9c8\ubaa8 \ud14c\uc2a4\ud2b8\uc758 5.7 \ubc0f 9.1 \u00b5m\uc640 \ube44\uad50\ud588\uc744 \ub54c \ub9e4\uc6b0 \ub192\uc740 \uc218\uce58\uc785\ub2c8\ub2e4. \uc774 \ud14c\uc2a4\ud2b8\ub294 \ud53c\uc2a4\ud1a4 \ub9c1-\uc2e4\ub9b0\ub354 \uc811\ucd09\ubd80\uc758 \uc801\uc808\ud55c \uc724\ud65c\uc774 \uc5bc\ub9c8\ub098 \uc911\uc694\ud55c\uc9c0 \ubcf4\uc5ec\uc90d\ub2c8\ub2e4. \ub9c8\ubaa8\uac00 \uc2ec\ud558\uba74 \uc724\ud65c\uc744 \ud558\uc9c0 \uc54a\uc544\ub3c4 \uc811\ucd09\uba74\uc774 \ube60\ub974\uac8c \uc190\uc0c1\ub418\uc5b4 \uc11c\ube44\uc2a4 \ud488\uc9c8\uc774 \ub3cc\uc774\ud0ac \uc218 \uc5c6\uc744 \uc815\ub3c4\ub85c \uc800\ud558\ub418\uace0 \uc5d4\uc9c4\uc774 \ud30c\uc190\ub420 \uc218\ub3c4 \uc788\uc2b5\ub2c8\ub2e4.<\/p><p>\u00a0<\/p><p style=\"margin: 0in; margin-bottom: .0001pt;\"><span style=\"font-family: 'Arial',sans-serif; color: #1c1e29;\">\u00a0<\/span><\/p><div style=\"text-align: center;\"><p><a href=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/05\/Figure-2-and-3.png\"><img decoding=\"async\" class=\"alignnone size-full wp-image-8350\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/05\/Figure-2-and-3.png\" alt=\"\" width=\"574\" height=\"847\" \/><\/a><\/p><p><a href=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/05\/Figure-4-and-Table-2.png\"><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-8351\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/05\/Figure-4-and-Table-2.png\" alt=\"\" width=\"671\" height=\"860\" \/><\/a><\/p><\/div><p style=\"text-align: left; color: #1b96cf; font-size: 24px; line-height: 30px;\"><strong><em>\uacb0\ub860<\/em><u><i><br \/><\/i><\/u><\/strong><\/p><div style=\"text-align: center;\"><a href=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/05\/Conclusion-Pic.png\"><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-8352\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/05\/Conclusion-Pic.png\" alt=\"\" width=\"699\" height=\"491\" \/><\/a><\/div><p>\ubcf8 \uc5f0\uad6c\uc5d0\uc11c\ub294 ASTM G77 \ud45c\uc900\uc5d0 \ub530\ub77c Block-on-Ring \ubaa8\ub4c8\uc744 \uc0ac\uc6a9\ud558\uc5ec \uac15\ucca0 \uae08\uc18d \ucee4\ud50c\uc758 \uc2ac\ub77c\uc774\ub529 \ub9c8\ubaa8 \uac70\ub3d9\uc744 \ud3c9\uac00\ud558\uae30 \uc704\ud574 Nanovea\uc758 \ub9c8\ucc30\uacc4\uac00 \uc5b4\ub5bb\uac8c \uc0ac\uc6a9\ub418\ub294\uc9c0 \ubcf4\uc5ec\uc90d\ub2c8\ub2e4. \uc724\ud65c\uc81c\ub294 \uc7ac\ub8cc \uc30d\uc758 \ub9c8\ubaa8 \ud2b9\uc131\uc5d0 \uc911\uc694\ud55c \uc5ed\ud560\uc744 \ud569\ub2c8\ub2e4. \ubbf8\ub124\ub784 \uc624\uc77c\uc740 H-30 \ube14\ub85d\uc758 \ub9c8\ubaa8\uc728\uc744 ~8\u00d710\u02c6, COF\ub97c ~90\ubc30 \uac10\uc18c\uc2dc\ud0b5\ub2c8\ub2e4. Nanovea \ub9c8\ucc30\uacc4\ub294 \ub2e4\uc591\ud55c \uae30\ub2a5\uc744 \uac16\ucd94\uace0 \uc788\uc5b4 \ub2e4\uc591\ud55c \uc724\ud65c, \uace0\uc628 \ubc0f \ub9c8\ucc30 \ubd80\uc2dd \uc870\uac74\uc5d0\uc11c \ub9c8\ubaa8 \uac70\ub3d9\uc744 \uce21\uc815\ud558\ub294 \ub370 \uc774\uc0c1\uc801\uc778 \ub3c4\uad6c\uc785\ub2c8\ub2e4.<\/p><p>Nanovea\uc758 \ud2b8\ub77c\uc774\ubcf4\ubbf8\ud130(Tribometer)\ub294 \ud558\ub098\uc758 \uc0ac\uc804 \ud1b5\ud569 \uc2dc\uc2a4\ud15c\uc5d0\uc11c \uc120\ud0dd\uc801\uc73c\ub85c \uc0ac\uc6a9\ud560 \uc218 \uc788\ub294 \uace0\uc628 \ub9c8\ubaa8, \uc724\ud65c \ubc0f \ub9c8\ucc30 \ubd80\uc2dd \ubaa8\ub4c8\uacfc \ud568\uaed8 ISO \ubc0f ASTM \uaddc\uaca9 \ud68c\uc804 \ubc0f \uc120\ud615 \ubaa8\ub4dc\ub97c \uc0ac\uc6a9\ud558\uc5ec \uc815\ud655\ud558\uace0 \ubc18\ubcf5 \uac00\ub2a5\ud55c \ub9c8\ubaa8 \ubc0f \ub9c8\ucc30 \ud14c\uc2a4\ud2b8\ub97c \uc81c\uacf5\ud569\ub2c8\ub2e4. Nanovea\uc758 \ud0c1\uc6d4\ud55c \uc81c\ud488\uad70\uc740 \uc587\uac70\ub098 \ub450\uaebc\uc6b4 \ucf54\ud305, \ubd80\ub4dc\ub7fd\uac70\ub098 \ub2e8\ub2e8\ud55c \ucf54\ud305, \ud544\ub984 \ubc0f \uae30\ud310\uc758 \ub9c8\ucc30 \ud2b9\uc131 \uc804\uccb4 \ubc94\uc704\ub97c \uacb0\uc815\ud558\ub294 \ub370 \uc774\uc0c1\uc801\uc778 \uc194\ub8e8\uc158\uc785\ub2c8\ub2e4.<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-d39e8a2 elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"d39e8a2\" data-element_type=\"section\" data-settings=\"{&quot;background_background&quot;:&quot;classic&quot;}\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-a5d0b1d\" data-id=\"a5d0b1d\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-1b82dad elementor-widget elementor-widget-heading\" data-id=\"1b82dad\" data-element_type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\"><b>\uc774\uc81c \uc560\ud50c\ub9ac\ucf00\uc774\uc158\uc5d0 \ub300\ud574 \uc774\uc57c\uae30\ud574 \ubcf4\uaca0\uc2b5\ub2c8\ub2e4.<\/b><\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-414bcdf live-chat elementor-align-center elementor-widget elementor-widget-button\" data-id=\"414bcdf\" data-element_type=\"widget\" data-widget_type=\"button.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<div class=\"elementor-button-wrapper\">\n\t\t\t\t\t<a class=\"elementor-button elementor-button-link elementor-size-md\" href=\"https:\/\/nanovea.com\/contact\/live-chat\/\" id=\"live-chat\">\n\t\t\t\t\t\t<span class=\"elementor-button-content-wrapper\">\n\t\t\t\t\t\t\t\t\t<span class=\"elementor-button-text\">\ub77c\uc774\ube0c \ucc44\ud305<\/span>\n\t\t\t\t\t<\/span>\n\t\t\t\t\t<\/a>\n\t\t\t\t<\/div>\n\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<\/div>","protected":false},"excerpt":{"rendered":"<p>IMPORTANCE OF BLOCK-ON-RING WEAR EVALUATION Sliding wear is the progressive loss of material that results from two materials sliding against each other at the contact area under load. It occurs inevitably in a wide variety of industries where machines and engines are in operation, including automotive, aerospace, oil &amp; gas and many others. Such sliding [&hellip;]<\/p>\n","protected":false},"author":1,"featured_media":11684,"comment_status":"open","ping_status":"open","sticky":false,"template":"","format":"standard","meta":{"_exactmetrics_skip_tracking":false,"_exactmetrics_sitenote_active":false,"_exactmetrics_sitenote_note":"","_exactmetrics_sitenote_category":0,"footnotes":""},"categories":[7,374,349,351,353,355,335,336],"tags":[],"class_list":["post-8344","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-application-notes","category-block-on-ring-tribology","category-laboratory-testing","category-profilometry-roughness-finish","category-profilometry-texture-grain","category-profilometry-volume-area","category-profilometry-testing","category-tribology-testing"],"_links":{"self":[{"href":"https:\/\/nanovea.com\/ko\/wp-json\/wp\/v2\/posts\/8344","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/nanovea.com\/ko\/wp-json\/wp\/v2\/posts"}],"about":[{"href":"https:\/\/nanovea.com\/ko\/wp-json\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"https:\/\/nanovea.com\/ko\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/nanovea.com\/ko\/wp-json\/wp\/v2\/comments?post=8344"}],"version-history":[{"count":19,"href":"https:\/\/nanovea.com\/ko\/wp-json\/wp\/v2\/posts\/8344\/revisions"}],"predecessor-version":[{"id":23411,"href":"https:\/\/nanovea.com\/ko\/wp-json\/wp\/v2\/posts\/8344\/revisions\/23411"}],"wp:featuredmedia":[{"embeddable":true,"href":"https:\/\/nanovea.com\/ko\/wp-json\/wp\/v2\/media\/11684"}],"wp:attachment":[{"href":"https:\/\/nanovea.com\/ko\/wp-json\/wp\/v2\/media?parent=8344"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"https:\/\/nanovea.com\/ko\/wp-json\/wp\/v2\/categories?post=8344"},{"taxonomy":"post_tag","embeddable":true,"href":"https:\/\/nanovea.com\/ko\/wp-json\/wp\/v2\/tags?post=8344"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}