{"id":8148,"date":"2020-04-08T15:27:56","date_gmt":"2020-04-08T15:27:56","guid":{"rendered":"https:\/\/nanovea.com\/?p=8148"},"modified":"2025-05-22T20:55:14","modified_gmt":"2025-05-22T20:55:14","slug":"%ed%91%9c%eb%a9%b4-%ec%b2%98%eb%a6%ac%eb%90%9c-%ea%b5%ac%eb%a6%ac%ec%84%a0%ec%9d%98-%eb%a7%88%eb%aa%a8-%eb%b0%8f-%ec%8a%a4%ed%81%ac%eb%9e%98%ec%b9%98-%ed%8f%89%ea%b0%80","status":"publish","type":"post","link":"https:\/\/nanovea.com\/ko\/wear-and-scratch-evaluation-of-surface-treated-copper-wire\/","title":{"rendered":"\ud45c\uba74 \ucc98\ub9ac\ub41c \uad6c\ub9ac\uc120\uc758 \ub9c8\ubaa8 \ubc0f \uc2a4\ud06c\ub798\uce58 \ud3c9\uac00"},"content":{"rendered":"<div data-elementor-type=\"wp-post\" data-elementor-id=\"8148\" class=\"elementor elementor-8148\" data-elementor-post-type=\"post\">\n\t\t\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-63d966a2 elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"63d966a2\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-7f9e98bf\" data-id=\"7f9e98bf\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-6a61ba79 elementor-widget elementor-widget-text-editor\" data-id=\"6a61ba79\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p style=\"text-align: left; color: #1b96cf; font-size: 24px;\">\uad6c\ub9ac\uc120\uc758 \ub9c8\ubaa8 \ubc0f \uc2a4\ud06c\ub798\uce58 \ud3c9\uac00\uc758 \uc911\uc694\uc131<strong><u><i><br \/><\/i><\/u><\/strong><\/p><p>\uad6c\ub9ac\ub294 \uc804\uc790\uc11d\uacfc \uc804\uc2e0\uc774 \ubc1c\uba85\ub41c \uc774\ub798 \uc804\uae30 \ubc30\uc120\uc5d0 \uc0ac\uc6a9\ub41c \uc624\ub79c \uc5ed\uc0ac\ub97c \uac00\uc9c0\uace0 \uc788\uc2b5\ub2c8\ub2e4. \uad6c\ub9ac\uc120\uc740 \ub0b4\uc2dd\uc131, \ub0a9\ub55c\uc131, \ucd5c\ub300 150\u00b0C\uc758 \uace0\uc628\uc5d0\uc11c\uc758 \uc131\ub2a5 \ub355\ubd84\uc5d0 \ud328\ub110, \uacc4\ub7c9\uae30, \ucef4\ud4e8\ud130, \uc5c5\ubb34\uc6a9 \uae30\uacc4 \ubc0f \uac00\uc804\uc81c\ud488\uacfc \uac19\uc740 \ub2e4\uc591\ud55c \uc804\uc790 \uc7a5\ube44\uc5d0 \uc801\uc6a9\ub429\ub2c8\ub2e4. \ucc44\uad74\ub41c \uad6c\ub9ac\uc758 \uc57d \uc808\ubc18\uc774 \uc804\uc120 \ubc0f \ucf00\uc774\ube14 \ub3c4\uccb4 \uc81c\uc870\uc5d0 \uc0ac\uc6a9\ub429\ub2c8\ub2e4.<\/p><p>\uad6c\ub9ac\uc120 \ud45c\uba74 \ud488\uc9c8\uc740 \uc560\ud50c\ub9ac\ucf00\uc774\uc158 \uc11c\ube44\uc2a4 \uc131\ub2a5\uacfc \uc218\uba85\uc5d0 \ub9e4\uc6b0 \uc911\uc694\ud569\ub2c8\ub2e4. \uc804\uc120\uc758 \ubbf8\uc138\ud55c \uacb0\ud568\uc740 \uacfc\ub3c4\ud55c \ub9c8\ubaa8, \uade0\uc5f4 \uc2dc\uc791 \ubc0f \uc804\ud30c, \uc804\ub3c4\ub3c4 \uac10\uc18c, \ub0a9\ub55c\uc131 \ubd80\uc801\ud569\uc73c\ub85c \uc774\uc5b4\uc9c8 \uc218 \uc788\uc2b5\ub2c8\ub2e4. \uad6c\ub9ac\uc120\uc758 \uc801\uc808\ud55c \ud45c\uba74 \ucc98\ub9ac\ub294 \uc640\uc774\uc5b4 \ub4dc\ub85c\uc789 \uc911\uc5d0 \ubc1c\uc0dd\ud558\ub294 \ud45c\uba74 \uacb0\ud568\uc744 \uc81c\uac70\ud558\uc5ec \ubd80\uc2dd, \uc2a4\ud06c\ub798\uce58 \ubc0f \ub0b4\ub9c8\ubaa8\uc131\uc744 \uac1c\uc120\ud569\ub2c8\ub2e4. \uad6c\ub9ac\uc120\uc744 \uc0ac\uc6a9\ud558\ub294 \ub9ce\uc740 \ud56d\uacf5\uc6b0\uc8fc \uc560\ud50c\ub9ac\ucf00\uc774\uc158\uc740 \uc608\uae30\uce58 \uc54a\uc740 \uc7a5\ube44 \uace0\uc7a5\uc744 \ubc29\uc9c0\ud558\uae30 \uc704\ud574 \uc81c\uc5b4\ub41c \ub3d9\uc791\uc774 \ud544\uc694\ud569\ub2c8\ub2e4. \uad6c\ub9ac\uc120 \ud45c\uba74\uc758 \ub0b4\ub9c8\ubaa8\uc131\uacfc \ub0b4\uc2a4\ud06c\ub798\uce58\uc131\uc744 \uc801\uc808\ud788 \ud3c9\uac00\ud558\uae30 \uc704\ud574\uc11c\ub294 \uc815\ub7c9\ud654\ub418\uace0 \uc2e0\ub8b0\ud560 \uc218 \uc788\ub294 \uce21\uc815\uc774 \ud544\uc694\ud569\ub2c8\ub2e4.<\/p><div>\u00a0<\/div><div>\u00a0<\/div><p>\u00a0<\/p><p style=\"text-align: left; color: #1b96cf; font-size: 24px;\">\uce21\uc815 \ubaa9\ud45c<\/p><p>\uc774 \uc560\ud50c\ub9ac\ucf00\uc774\uc158\uc5d0\uc11c\ub294 \ub2e4\uc591\ud55c \uad6c\ub9ac\uc120 \ud45c\uba74 \ucc98\ub9ac\uc758 \uc81c\uc5b4\ub41c \ub9c8\ubaa8 \ud504\ub85c\uc138\uc2a4\ub97c \uc2dc\ubbac\ub808\uc774\uc158\ud569\ub2c8\ub2e4. <a href=\"https:\/\/nanovea.com\/scratch-tester\/\">\uc2a4\ud06c\ub798\uce58 \ud14c\uc2a4\ud2b8<\/a> \ucc98\ub9ac\ub41c \ud45c\uba74\uce35\uc5d0 \ud30c\uc190\uc744 \uc77c\uc73c\ud0a4\ub294 \ub370 \ud544\uc694\ud55c \ud558\uc911\uc744 \uce21\uc815\ud569\ub2c8\ub2e4. \uc774\ubc88 \uc5f0\uad6c\uc5d0\uc11c\ub294 Nanovea\ub97c \uc18c\uac1c\ud569\ub2c8\ub2e4. <a href=\"https:\/\/nanovea.com\/tribometers\/\">\ud2b8\ub77c\uc774\ubcf4\ubbf8\ud130 <\/a>\uadf8\ub9ac\uace0 <a href=\"https:\/\/nanovea.com\/mechanical-testers\/\">\uae30\uacc4 \ud14c\uc2a4\ud130<\/a> \uc804\uc120\uc758 \ud3c9\uac00 \ubc0f \ud488\uc9c8 \uad00\ub9ac\ub97c \uc704\ud55c \uc774\uc0c1\uc801\uc778 \ub3c4\uad6c\uc785\ub2c8\ub2e4.<\/p><div style=\"text-align: center;\">\u00a0<\/div><p>\u00a0<\/p><p style=\"text-align: left; color: #1b96cf; font-size: 24px;\">\ud14c\uc2a4\ud2b8 \uc808\ucc28 \ubc0f \ubc29\ubc95<strong><u><i><br \/><\/i><\/u><\/strong><\/p><p>\uad6c\ub9ac \uc640\uc774\uc5b4(\uc640\uc774\uc5b4 A \ubc0f \uc640\uc774\uc5b4 B)\uc5d0 \ub300\ud55c \ub450 \uac00\uc9c0 \ub2e4\ub978 \ud45c\uba74 \ucc98\ub9ac\uc758 \ub9c8\ucc30 \uacc4\uc218(COF)\uc640 \ub0b4\ub9c8\ubaa8\uc131\uc740 \uc120\ud615 \uc655\ubcf5 \ub9c8\ubaa8 \ubaa8\ub4c8\uc744 \uc0ac\uc6a9\ud558\ub294 Nanovea \ub9c8\ucc30\uacc4\ub85c \ud3c9\uac00\ub418\uc5c8\uc2b5\ub2c8\ub2e4. Al2O\u2083 \ubcfc(\uc9c1\uacbd 6mm)\uc774 \uc774 \uc751\uc6a9 \ubd84\uc57c\uc5d0 \uc0ac\uc6a9\ub418\ub294 \uce74\uc6b4\ud130 \uc7ac\ub8cc\uc785\ub2c8\ub2e4. \ub9c8\ubaa8 \ud2b8\ub799\uc740 Nanovea\ub97c \uc0ac\uc6a9\ud558\uc5ec \uac80\uc0ac\ub418\uc5c8\uc2b5\ub2c8\ub2e4. <a href=\"https:\/\/nanovea.com\/profilometers\/\">3D \ube44\uc811\ucd09 \ud504\ub85c\ud30c\uc77c\ub85c\ubbf8\ud130<\/a>. \ud14c\uc2a4\ud2b8 \ub9e4\uac1c\ubcc0\uc218\ub294 \ud45c 1\uc5d0 \uc694\uc57d\ub418\uc5b4 \uc788\uc2b5\ub2c8\ub2e4.<\/p><p>\uc774 \uc5f0\uad6c\uc5d0\uc11c\ub294 \uce74\uc6b4\ud130 \uc7ac\ub8cc\ub85c \ub9e4\ub044\ub7ec\uc6b4 Al\u2082O\u2083 \ubcfc\uc744 \uc608\ub85c \uc0ac\uc6a9\ud588\uc2b5\ub2c8\ub2e4. \uc2e4\uc81c \uc801\uc6a9 \uc0c1\ud669\uc744 \uc2dc\ubbac\ub808\uc774\uc158\ud558\uae30 \uc704\ud574 \ub9de\ucda4\ud615 \ud53d\uc2a4\ucc98\ub97c \uc0ac\uc6a9\ud558\uc5ec \ubaa8\uc591\uacfc \ud45c\uba74 \ub9c8\uac10\uc774 \ub2e4\ub978 \ubaa8\ub4e0 \uace0\uccb4 \uc18c\uc7ac\ub97c \uc801\uc6a9\ud560 \uc218 \uc788\uc2b5\ub2c8\ub2e4.<\/p><p><a href=\"https:\/\/nanovea.com\/wp-content\/uploads\/2020\/04\/Table-1.png\"><img fetchpriority=\"high\" decoding=\"async\" class=\"alignnone size-full wp-image-8149\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2020\/04\/Table-1.png\" alt=\"\" width=\"1245\" height=\"801\" \/><\/a><\/p><div style=\"text-align: center;\">\u00a0<\/div><p>\u00a0<\/p><div>\ub85c\ud06c\uc6f0 C \ub2e4\uc774\uc544\ubaac\ub4dc \uc2a4\ud0c0\uc77c\ub7ec\uc2a4(\ubc18\uacbd 100\u03bcm)\uac00 \uc7a5\ucc29\ub41c \ub098\ub178\ubca0\uc544\uc758 \uae30\uacc4\uc2dd \ud14c\uc2a4\ud130\ub294 \ub9c8\uc774\ud06c\ub85c \uc2a4\ud06c\ub798\uce58 \ubaa8\ub4dc\ub97c \uc0ac\uc6a9\ud558\uc5ec \ucf54\ud305\ub41c \uc804\uc120\uc5d0 \ub300\ud574 \ud504\ub85c\uadf8\ub808\uc2dc\ube0c \ud558\uc911 \uc2a4\ud06c\ub798\uce58 \ud14c\uc2a4\ud2b8\ub97c \uc218\ud589\ud588\uc2b5\ub2c8\ub2e4. \uc2a4\ud06c\ub798\uce58 \ud14c\uc2a4\ud2b8 \ud30c\ub77c\ubbf8\ud130\uc640 \ud301 \ud615\uc0c1\uc740 \ud45c 2\uc5d0 \ub098\uc640 \uc788\uc2b5\ub2c8\ub2e4.<\/div><div>\u00a0<\/div><p>\u00a0<\/p><div><a href=\"https:\/\/nanovea.com\/wp-content\/uploads\/2020\/04\/Table-2.png\"><img decoding=\"async\" class=\"alignnone size-full wp-image-8150\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2020\/04\/Table-2.png\" alt=\"\" width=\"874\" height=\"809\" \/><\/a><\/div><div>\u00a0<\/div><p>\u00a0<\/p><p style=\"text-align: left; color: #1b96cf; font-size: 24px;\">\uacb0\uacfc \ubc0f \ud1a0\ub860<u><i><\/i><\/u><\/p><p><strong>\uad6c\ub9ac\uc120\uc758 \ub9c8\ubaa8:<\/strong><\/p><p>\uadf8\ub9bc 2\ub294 \ub9c8\ubaa8 \ud14c\uc2a4\ud2b8 \uc911 \uad6c\ub9ac\uc120\uc758 COF \ubcc0\ud654\ub97c \ubcf4\uc5ec\uc90d\ub2c8\ub2e4. \uc640\uc774\uc5b4 A\ub294 \ub9c8\ubaa8 \ud14c\uc2a4\ud2b8 \ub0b4\ub0b4 ~0.4\uc758 \uc548\uc815\uc801\uc778 COF\ub97c \ubcf4\uc774\ub294 \ubc18\uba74, \uc640\uc774\uc5b4 B\ub294 \ucc98\uc74c 100\ud68c\uc804 \ub3d9\uc548 ~0.35\uc758 COF\ub97c \ubcf4\uc774\ub2e4\uac00 \uc810\ucc28 ~0.4\uae4c\uc9c0 \uc99d\uac00\ud569\ub2c8\ub2e4.<\/p><p style=\"margin: 0in; margin-bottom: .0001pt;\"><span style=\"font-family: 'Arial',sans-serif;\"><a href=\"https:\/\/nanovea.com\/wp-content\/uploads\/2020\/04\/Figure-2.png\"><img decoding=\"async\" class=\"alignnone size-full wp-image-8151\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2020\/04\/Figure-2.png\" alt=\"\" width=\"839\" height=\"709\" \/><\/a><\/span><\/p><p>\u00a0<\/p><p style=\"margin: 0in; margin-bottom: .0001pt;\"><span style=\"font-family: 'Arial',sans-serif; color: #1c1e29;\">\uadf8\ub9bc 3\uc740 \ud14c\uc2a4\ud2b8 \ud6c4 \uad6c\ub9ac\uc120\uc758 \ub9c8\ubaa8 \ud2b8\ub799\uc744 \ube44\uad50\ud55c \uac83\uc785\ub2c8\ub2e4. \ub098\ub178\ube44\uc544\uc758 3D \ube44\uc811\ucd09\uc2dd \ud504\ub85c\ud30c\uc77c\ub85c\ubbf8\ud130\ub294 \ub9c8\ubaa8 \ud2b8\ub799\uc758 \uc138\ubd80\uc801\uc778 \ud615\ud0dc\uc5d0 \ub300\ud55c \ud0c1\uc6d4\ud55c \ubd84\uc11d\uc744 \uc81c\uacf5\ud588\uc2b5\ub2c8\ub2e4. \ub9c8\ubaa8 \uba54\ucee4\ub2c8\uc998\uc5d0 \ub300\ud55c \uadfc\ubcf8\uc801\uc778 \uc774\ud574\ub97c \uc81c\uacf5\ud568\uc73c\ub85c\uc368 \ub9c8\ubaa8 \ud2b8\ub799\uc758 \uc591\uc744 \uc9c1\uc811\uc801\uc774\uace0 \uc815\ud655\ud558\uac8c \uce21\uc815\ud560 \uc218 \uc788\uc2b5\ub2c8\ub2e4. \uc640\uc774\uc5b4 B\uc758 \ud45c\uba74\uc740 600\ud68c \ud68c\uc804 \ub9c8\ubaa8 \ud14c\uc2a4\ud2b8 \ud6c4 \uc0c1\ub2f9\ud55c \ub9c8\ubaa8 \ud2b8\ub799 \uc190\uc0c1\uc744 \uc785\uc5c8\uc2b5\ub2c8\ub2e4. \ud504\ub85c\ud30c\uc77c\ub85c\ubbf8\ud130 3D \ubdf0\ub294 \uc640\uc774\uc5b4 B\uc758 \ud45c\uba74 \ucc98\ub9ac\uce35\uc774 \uc644\uc804\ud788 \uc81c\uac70\ub418\uc5b4 \ub9c8\ubaa8 \uacfc\uc815\uc774 \uc0c1\ub2f9\ud788 \ube68\ub77c\uc9c4 \uac83\uc744 \ubcf4\uc5ec\uc90d\ub2c8\ub2e4. \uc774\ub85c \uc778\ud574 \uad6c\ub9ac \uae30\ud310\uc774 \ub178\ucd9c\ub41c \uc640\uc774\uc5b4 B\uc5d0 \ud3c9\ud3c9\ud55c \ub9c8\ubaa8 \ud2b8\ub799\uc774 \ub0a8\uc558\uc2b5\ub2c8\ub2e4. \uc774\ub85c \uc778\ud574 B \uc640\uc774\uc5b4\uac00 \uc0ac\uc6a9\ub418\ub294 \uc804\uae30 \uc7a5\ube44\uc758 \uc218\uba85\uc774 \ud06c\uac8c \ub2e8\ucd95\ub420 \uc218 \uc788\uc2b5\ub2c8\ub2e4. \uc774\uc5d0 \ube44\ud574 \uc804\uc120 A\ub294 \ud45c\uba74\uc5d0 \uc595\uc740 \ub9c8\ubaa8 \ud2b8\ub799\uc774 \ub098\ud0c0\ub098 \ube44\uad50\uc801 \uac00\ubcbc\uc6b4 \ub9c8\ubaa8\ub97c \ubcf4\uc600\uc2b5\ub2c8\ub2e4. \uc804\uc120 A\uc758 \ud45c\uba74 \ucc98\ub9ac\ub41c \uce35\uc740 \ub3d9\uc77c\ud55c \uc870\uac74\uc5d0\uc11c \uc804\uc120 B\uc758 \uce35\ucc98\ub7fc \uc81c\uac70\ub418\uc9c0 \uc54a\uc558\uc2b5\ub2c8\ub2e4.<\/span><\/p><p><a href=\"https:\/\/nanovea.com\/wp-content\/uploads\/2020\/04\/Wire-A.png\"><img loading=\"lazy\" decoding=\"async\" class=\"alignnone wp-image-8152\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2020\/04\/Wire-A.png\" alt=\"\" width=\"1048\" height=\"544\" \/><\/a><\/p><p><a href=\"https:\/\/nanovea.com\/wp-content\/uploads\/2020\/04\/Wire-B.png\"><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-8153\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2020\/04\/Wire-B.png\" alt=\"\" width=\"1051\" height=\"616\" \/><\/a><\/p><p><strong>\uad6c\ub9ac\uc120 \ud45c\uba74\uc758 \uc2a4\ud06c\ub798\uce58 \ubc29\uc9c0:<\/strong><\/p><p>\uadf8\ub9bc 4\ub294 \ud14c\uc2a4\ud2b8 \ud6c4 \uc804\uc120\uc758 \uc2a4\ud06c\ub798\uce58 \ud2b8\ub799\uc744 \ubcf4\uc5ec\uc90d\ub2c8\ub2e4. \uc804\uc120 A\uc758 \ubcf4\ud638\uce35\uc740 \ub9e4\uc6b0 \uc6b0\uc218\ud55c \uc2a4\ud06c\ub798\uce58 \uc800\ud56d\uc131\uc744 \ubcf4\uc5ec\uc90d\ub2c8\ub2e4. \uc774 \uc804\uc120\uc740 ~12.6N\uc758 \ud558\uc911\uc5d0\uc11c \ubc15\ub9ac\ub41c \ubc18\uba74, B \uc804\uc120\uc758 \ubcf4\ud638\uce35\uc740 ~1.0N\uc758 \ud558\uc911\uc5d0\uc11c \ubc15\ub9ac\ub418\uc5c8\uc2b5\ub2c8\ub2e4. \uc774\ub7ec\ud55c \uc804\uc120\uc758 \uc2a4\ud06c\ub798\uce58 \uc800\ud56d\uc131\uc5d0 \ub300\ud55c \uc0c1\ub2f9\ud55c \ucc28\uc774\ub294 \uc804\uc120 A\uc758 \ub0b4\ub9c8\ubaa8\uc131\uc774 \uc0c1\ub2f9\ud788 \ud5a5\uc0c1\ub41c \ub9c8\ubaa8 \uc131\ub2a5\uc5d0 \uc601\ud5a5\uc744 \ubbf8\uce69\ub2c8\ub2e4. \uadf8\ub9bc 5\uc5d0 \ud45c\uc2dc\ub41c \uc2a4\ud06c\ub798\uce58 \ud14c\uc2a4\ud2b8 \uc911 \uc815\uc0c1 \ud798, COF \ubc0f \uae4a\uc774\uc758 \ubcc0\ud654\ub294 \ud14c\uc2a4\ud2b8 \uc911 \ucf54\ud305 \uc2e4\ud328\uc5d0 \ub300\ud55c \ub354 \ub9ce\uc740 \ud1b5\ucc30\ub825\uc744 \uc81c\uacf5\ud569\ub2c8\ub2e4.<\/p><p><a href=\"https:\/\/nanovea.com\/wp-content\/uploads\/2020\/04\/Figure-4.png\"><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-8155\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2020\/04\/Figure-4.png\" alt=\"\" width=\"959\" height=\"559\" \/><\/a><\/p><p><a href=\"https:\/\/nanovea.com\/wp-content\/uploads\/2020\/04\/Figure-5.png\"><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-8154\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2020\/04\/Figure-5.png\" alt=\"\" width=\"987\" height=\"891\" \/><\/a><\/p><p style=\"text-align: left; color: #1b96cf; font-size: 24px;\">\uacb0\ub860<\/p><p><a href=\"https:\/\/nanovea.com\/wp-content\/uploads\/2020\/04\/electric-948208_1920.jpg\"><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-8159\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2020\/04\/electric-948208_1920.jpg\" alt=\"\" width=\"1920\" height=\"1080\" \/><\/a><\/p><p>\uc774 \ub300\uc870 \uc5f0\uad6c\uc5d0\uc11c\ub294 \ud45c\uba74 \ucc98\ub9ac\ub41c \uad6c\ub9ac\uc120\uc758 \ub0b4\ub9c8\ubaa8\uc131\uc744 \uc815\ub7c9\uc801\uc73c\ub85c \ud3c9\uac00\ud558\ub294 \ub098\ub178\ubca0\uc544\uc758 \ud2b8\ub77c\uc774\ubcf4\ubbf8\ud130\uc640 \uad6c\ub9ac\uc120\uc758 \uc2a4\ud06c\ub798\uce58 \uc800\ud56d\uc131\uc744 \uc2e0\ub8b0\uc131 \uc788\uac8c \ud3c9\uac00\ud558\ub294 \ub098\ub178\ubca0\uc544\uc758 \uae30\uacc4\uc2dd \ud14c\uc2a4\ud130\ub97c \uc120\ubcf4\uc600\uc2b5\ub2c8\ub2e4. \uc640\uc774\uc5b4 \ud45c\uba74 \ucc98\ub9ac\ub294 \uc640\uc774\uc5b4\uc758 \uc218\uba85 \ub3d9\uc548 \ud2b8\ub77c\uc774\ubcf4-\uae30\uacc4\uc801 \ud2b9\uc131\uc5d0 \uc911\uc694\ud55c \uc5ed\ud560\uc744 \ud569\ub2c8\ub2e4. \uc640\uc774\uc5b4 A\uc758 \uc801\uc808\ud55c \ud45c\uba74 \ucc98\ub9ac\ub294 \uac70\uce5c \ud658\uacbd\uc5d0\uc11c \uc804\uc120\uc758 \uc131\ub2a5\uacfc \uc218\uba85\uc5d0 \uc911\uc694\ud55c \ub9c8\ubaa8 \ubc0f \uae01\ud798 \uc800\ud56d\uc131\uc744 \ud06c\uac8c \ud5a5\uc0c1\uc2dc\ud0b5\ub2c8\ub2e4.<\/p><p>\ub098\ub178\ubca0\uc544\uc758 \ud2b8\ub77c\uc774\ubcf4\ubbf8\ud130\ub294 ISO \ubc0f ASTM\uc744 \uc900\uc218\ud558\ub294 \ud68c\uc804 \ubc0f \uc120\ud615 \ubaa8\ub4dc\ub97c \uc0ac\uc6a9\ud558\uc5ec \uc815\ubc00\ud558\uace0 \ubc18\ubcf5 \uac00\ub2a5\ud55c \ub9c8\ubaa8 \ubc0f \ub9c8\ucc30 \ud14c\uc2a4\ud2b8\ub97c \uc81c\uacf5\ud558\uba70, \ud558\ub098\uc758 \uc0ac\uc804 \ud1b5\ud569\ub41c \uc2dc\uc2a4\ud15c\uc5d0\uc11c \uace0\uc628 \ub9c8\ubaa8, \uc724\ud65c \ubc0f \ud2b8\ub9ac\ubcf4 \ubd80\uc2dd \ubaa8\ub4c8\uc744 \uc635\uc158\uc73c\ub85c \uc0ac\uc6a9\ud560 \uc218 \uc788\uc2b5\ub2c8\ub2e4. \ub098\ub178\ube44\uc544\uc758 \ub3c5\ubcf4\uc801\uc778 \uc81c\ud488\uad70\uc740 \uc587\uac70\ub098 \ub450\uaebc\uc6b4, \uc5f0\uc9c8 \ub610\ub294 \uacbd\uc9c8 \ucf54\ud305, \ud544\ub984 \ubc0f \uae30\ud310\uc758 \ubaa8\ub4e0 \ub9c8\ucc30 \ud2b9\uc131\uc744 \uce21\uc815\ud558\ub294 \ub370 \uc774\uc0c1\uc801\uc778 \uc194\ub8e8\uc158\uc785\ub2c8\ub2e4.<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-4298afa elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"4298afa\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-e45e6d1\" data-id=\"e45e6d1\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-17b94b6 elementor-widget elementor-widget-heading\" data-id=\"17b94b6\" data-element_type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\">\ube44\uc2b7\ud55c \uc560\ud50c\ub9ac\ucf00\uc774\uc158\uc774 \uc788\uc73c\uc2e0\uac00\uc694?<\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-0670c7e elementor-align-justify open-chat elementor-widget elementor-widget-button\" data-id=\"0670c7e\" data-element_type=\"widget\" data-widget_type=\"button.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<div class=\"elementor-button-wrapper\">\n\t\t\t\t\t<a class=\"elementor-button elementor-size-sm\" role=\"button\">\n\t\t\t\t\t\t<span class=\"elementor-button-content-wrapper\">\n\t\t\t\t\t\t\t\t\t<span class=\"elementor-button-text\">\uc9c0\uae08 \uc804\ubb38\uac00\uc640 \uc0c1\ub2f4\ud558\uc138\uc694<\/span>\n\t\t\t\t\t<\/span>\n\t\t\t\t\t<\/a>\n\t\t\t\t<\/div>\n\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-bde5855 elementor-align-justify button-quote elementor-widget elementor-widget-button\" data-id=\"bde5855\" data-element_type=\"widget\" data-widget_type=\"button.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<div class=\"elementor-button-wrapper\">\n\t\t\t\t\t<a class=\"elementor-button elementor-button-link elementor-size-sm\" href=\"https:\/\/nanovea.com\/contact-sales-form\/\" id=\"button-quote-bottom\">\n\t\t\t\t\t\t<span class=\"elementor-button-content-wrapper\">\n\t\t\t\t\t\t\t\t\t<span class=\"elementor-button-text\">\uac00\uaca9 \ubc0f \uc138\ubd80 \uc815\ubcf4 \ube60\ub974\uac8c \ud655\uc778\ud558\uae30<\/span>\n\t\t\t\t\t<\/span>\n\t\t\t\t\t<\/a>\n\t\t\t\t<\/div>\n\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<\/div>","protected":false},"excerpt":{"rendered":"","protected":false},"author":1,"featured_media":11689,"comment_status":"open","ping_status":"open","sticky":false,"template":"","format":"standard","meta":{"_exactmetrics_skip_tracking":false,"_exactmetrics_sitenote_active":false,"_exactmetrics_sitenote_note":"","_exactmetrics_sitenote_category":0,"footnotes":""},"categories":[7,349,372,337,350,353,335,345,346,336],"tags":[],"class_list":["post-8148","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-application-notes","category-laboratory-testing","category-linear-tribology","category-mechanical-testing","category-profilometry-geometry-shape","category-profilometry-texture-grain","category-profilometry-testing","category-scratch-testing-adhesive-failure","category-scratch-testing-cohesive-failure","category-tribology-testing"],"_links":{"self":[{"href":"https:\/\/nanovea.com\/ko\/wp-json\/wp\/v2\/posts\/8148","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/nanovea.com\/ko\/wp-json\/wp\/v2\/posts"}],"about":[{"href":"https:\/\/nanovea.com\/ko\/wp-json\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"https:\/\/nanovea.com\/ko\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/nanovea.com\/ko\/wp-json\/wp\/v2\/comments?post=8148"}],"version-history":[{"count":37,"href":"https:\/\/nanovea.com\/ko\/wp-json\/wp\/v2\/posts\/8148\/revisions"}],"predecessor-version":[{"id":24779,"href":"https:\/\/nanovea.com\/ko\/wp-json\/wp\/v2\/posts\/8148\/revisions\/24779"}],"wp:featuredmedia":[{"embeddable":true,"href":"https:\/\/nanovea.com\/ko\/wp-json\/wp\/v2\/media\/11689"}],"wp:attachment":[{"href":"https:\/\/nanovea.com\/ko\/wp-json\/wp\/v2\/media?parent=8148"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"https:\/\/nanovea.com\/ko\/wp-json\/wp\/v2\/categories?post=8148"},{"taxonomy":"post_tag","embeddable":true,"href":"https:\/\/nanovea.com\/ko\/wp-json\/wp\/v2\/tags?post=8148"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}