{"id":20021,"date":"2022-05-27T22:23:41","date_gmt":"2022-05-27T22:23:41","guid":{"rendered":"https:\/\/nanovea.com\/?p=20021"},"modified":"2024-10-08T16:52:33","modified_gmt":"2024-10-08T16:52:33","slug":"%ec%82%b0%ec%97%85%ec%9a%a9-%ec%bd%94%ed%8c%85-%ec%8a%a4%ed%81%ac%eb%9e%98%ec%b9%98-%eb%b0%8f-%eb%a7%88%eb%aa%a8-%ed%8f%89%ea%b0%80","status":"publish","type":"post","link":"https:\/\/nanovea.com\/ko\/industrial-coatings-scratch-and-wear-evaluation\/","title":{"rendered":"\uc0b0\uc5c5\uc6a9 \ucf54\ud305 \uc2a4\ud06c\ub798\uce58 \ubc0f \ub9c8\ubaa8 \ud3c9\uac00"},"content":{"rendered":"<div data-elementor-type=\"wp-post\" data-elementor-id=\"20021\" class=\"elementor elementor-20021\" data-elementor-post-type=\"post\">\n\t\t\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-7ec3d48 elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"7ec3d48\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-c477953\" data-id=\"c477953\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-cec2c6e elementor-widget elementor-widget-heading\" data-id=\"cec2c6e\" data-element_type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h1 class=\"elementor-heading-title elementor-size-default\">\uc0b0\uc5c5\uc6a9 \ucf54\ud305<\/h1>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-d107f9b elementor-widget elementor-widget-heading\" data-id=\"d107f9b\" data-element_type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\">\ud2b8\ub77c\uc774\ubcf4\ubbf8\ud130\ub97c \uc0ac\uc6a9\ud55c \uc2a4\ud06c\ub798\uce58 \ubc0f \ub9c8\ubaa8 \ud3c9\uac00<\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-73c118d elementor-widget elementor-widget-image\" data-id=\"73c118d\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img fetchpriority=\"high\" decoding=\"async\" width=\"768\" height=\"242\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2022\/05\/Industrial-Coatings-Evaluation.jpg\" class=\"attachment-medium_large size-medium_large wp-image-20025\" alt=\"\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-97cc106 elementor-widget elementor-widget-heading\" data-id=\"97cc106\" data-element_type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\">\uc791\uc131\uc790<\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-95aa94e elementor-widget elementor-widget-heading\" data-id=\"95aa94e\" data-element_type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\">DUANJIE LI, \ubc15\uc0ac \ubc0f \uc548\ub4dc\ub808\uc544 \ud5e4\ub974\ub9cc(ANDREA HERRMANN)<\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-c14383d elementor-widget elementor-widget-spacer\" data-id=\"c14383d\" data-element_type=\"widget\" data-widget_type=\"spacer.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t<div class=\"elementor-spacer\">\n\t\t\t<div class=\"elementor-spacer-inner\"><\/div>\n\t\t<\/div>\n\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-753c1f3 elementor-section-content-middle elementor-reverse-mobile elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"753c1f3\" data-element_type=\"section\" data-settings=\"{&quot;background_background&quot;:&quot;classic&quot;}\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-top-column elementor-element elementor-element-f2074e4 elementor-hidden-phone\" data-id=\"f2074e4\" data-element_type=\"column\" data-settings=\"{&quot;background_background&quot;:&quot;classic&quot;}\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-c0f91f8 elementor-widget elementor-widget-spacer\" data-id=\"c0f91f8\" data-element_type=\"widget\" data-widget_type=\"spacer.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t<div class=\"elementor-spacer\">\n\t\t\t<div class=\"elementor-spacer-inner\"><\/div>\n\t\t<\/div>\n\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-top-column elementor-element elementor-element-b259d86\" data-id=\"b259d86\" data-element_type=\"column\" data-settings=\"{&quot;background_background&quot;:&quot;classic&quot;}\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-62f2a44 elementor-widget elementor-widget-heading\" data-id=\"62f2a44\" data-element_type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\">\uc18c\uac1c<\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-9ab0009 elementor-widget elementor-widget-text-editor\" data-id=\"9ab0009\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p>\uc544\ud06c\ub9b4 \uc6b0\ub808\ud0c4 \ud398\uc778\ud2b8\ub294 \ubc14\ub2e5 \ud398\uc778\ud2b8, \uc790\ub3d9\ucc28 \ud398\uc778\ud2b8 \ub4f1 \ub2e4\uc591\ud55c \uc0b0\uc5c5 \ubd84\uc57c\uc5d0\uc11c \ub110\ub9ac \uc0ac\uc6a9\ub418\ub294 \uc18d\uac74\uc131 \ubcf4\ud638 \ucf54\ud305\uc758 \uc77c\uc885\uc785\ub2c8\ub2e4. \ubc14\ub2e5 \ud398\uc778\ud2b8\ub85c \uc0ac\uc6a9\ud558\uba74 \ubcf4\ub3c4, \uc5f0\uc11d \ubc0f \uc8fc\ucc28\uc7a5\uacfc \uac19\uc774 \ubc1c\uacfc \uace0\ubb34 \ubc14\ud034\uac00 \ub9ce\uc774 \ub2e4\ub2c8\ub294 \uad6c\uc5ed\uc5d0 \uc0ac\uc6a9\ud560 \uc218 \uc788\uc2b5\ub2c8\ub2e4.<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-d440447 elementor-widget elementor-widget-heading\" data-id=\"d440447\" data-element_type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\">\ud488\uc9c8 \uad00\ub9ac\ub97c \uc704\ud55c \uc2a4\ud06c\ub798\uce58 \ubc0f \ub9c8\ubaa8 \ud14c\uc2a4\ud2b8\uc758 \uc911\uc694\uc131<\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-966ab4d elementor-widget elementor-widget-text-editor\" data-id=\"966ab4d\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p>\uc804\ud1b5\uc801\uc73c\ub85c \ud14c\uc774\ubc84 \ub9c8\ubaa8 \ud14c\uc2a4\ud2b8\ub294 ASTM D4060 \ud45c\uc900\uc5d0 \ub530\ub77c \uc544\ud06c\ub9b4 \uc6b0\ub808\ud0c4 \ubc14\ub2e5 \ud398\uc778\ud2b8\uc758 \ub0b4\ub9c8\ubaa8\uc131\uc744 \ud3c9\uac00\ud558\uae30 \uc704\ud574 \uc218\ud589\ub418\uc5c8\uc2b5\ub2c8\ub2e4. \uadf8\ub7ec\ub098 \ud45c\uc900\uc5d0 \uc5b8\uae09\ub41c \ubc14\uc640 \uac19\uc774 \"\uc77c\ubd80 \uc7ac\ub8cc\uc758 \uacbd\uc6b0, \ud14c\uc774\ubc84 \uc5f0\ub9c8\uae30\ub97c \uc0ac\uc6a9\ud55c \ub9c8\ubaa8 \ud14c\uc2a4\ud2b8\ub294 \ud14c\uc2a4\ud2b8 \uc911 \ud720\uc758 \uc5f0\ub9c8 \ud2b9\uc131 \ubcc0\ud654\ub85c \uc778\ud574 \ud3b8\ucc28\uac00 \ubc1c\uc0dd\ud560 \uc218 \uc788\uc2b5\ub2c8\ub2e4.\"1 \uc774\ub85c \uc778\ud574 \ud14c\uc2a4\ud2b8 \uacb0\uacfc\uc758 \uc7ac\ud604\uc131\uc774 \ub5a8\uc5b4\uc9c0\uace0 \ub2e4\ub978 \uc2e4\ud5d8\uc2e4\uc5d0\uc11c \ubcf4\uace0\ub41c \uac12\uc744 \ube44\uad50\ud558\uae30 \uc5b4\ub824\uc6b8 \uc218 \uc788\uc2b5\ub2c8\ub2e4. \ub610\ud55c \ud14c\uc774\ud37c \ub9c8\ubaa8 \ud14c\uc2a4\ud2b8\uc5d0\uc11c \ub0b4\ub9c8\ubaa8\uc131\uc740 \uc9c0\uc815\ub41c \ub9c8\ubaa8 \uc0ac\uc774\ud074 \ud69f\uc218\uc5d0\uc11c \ubb34\uac8c\uc758 \uc190\uc2e4\ub85c \uacc4\uc0b0\ub429\ub2c8\ub2e4. \uadf8\ub7ec\ub098 \uc544\ud06c\ub9b4 \uc6b0\ub808\ud0c4 \ubc14\ub2e5 \ud398\uc778\ud2b8\uc758 \uad8c\uc7a5 \uac74\uc870\ub9c9 \ub450\uaed8\ub294 37.5-50 \u03bcm2\uc785\ub2c8\ub2e4.<\/p><p>\ud14c\uc774\ubc84 \uc5f0\ub9c8\uae30\uc758 \uacf5\uaca9\uc801\uc778 \ub9c8\ubaa8 \uacf5\uc815\uc740 \uc544\ud06c\ub9b4 \uc6b0\ub808\ud0c4 \ucf54\ud305\uc744 \ube60\ub974\uac8c \ub9c8\ubaa8\uc2dc\ud0a4\uace0 \uae30\ud310\uc5d0 \uc9c8\ub7c9 \uc190\uc2e4\uc744 \uc77c\uc73c\ucf1c \ud398\uc778\ud2b8 \uc911\ub7c9 \uc190\uc2e4 \uacc4\uc0b0\uc5d0 \uc0c1\ub2f9\ud55c \uc624\ub958\ub97c \ucd08\ub798\ud560 \uc218 \uc788\uc2b5\ub2c8\ub2e4. \ub9c8\ubaa8 \ud14c\uc2a4\ud2b8 \uc911 \ud398\uc778\ud2b8\uc5d0 \uc5f0\ub9c8 \uc785\uc790\ub97c \uc8fc\uc785\ud558\ub294 \uac83\ub3c4 \uc624\ub958\uc758 \uc6d0\uc778\uc774 \ub429\ub2c8\ub2e4. \ub530\ub77c\uc11c \ud398\uc778\ud2b8\uc758 \uc7ac\ud604 \uac00\ub2a5\ud55c \ub9c8\ubaa8 \ud3c9\uac00\ub97c \ubcf4\uc7a5\ud558\ub824\uba74 \uc798 \uc81c\uc5b4\ub418\uace0 \uc815\ub7c9\ud654 \uac00\ub2a5\ud558\uba70 \uc2e0\ub8b0\ud560 \uc218 \uc788\ub294 \uce21\uc815\uc774 \uc911\uc694\ud569\ub2c8\ub2e4. \ub610\ud55c <a href=\"https:\/\/nanovea.com\/scratch-tester\/\">\uc2a4\ud06c\ub798\uce58 \ud14c\uc2a4\ud2b8<\/a> \ub97c \uc0ac\uc6a9\ud558\uba74 \uc2e4\uc81c \uc751\uc6a9 \ubd84\uc57c\uc5d0\uc11c \uc870\uae30\uc5d0 \uc811\ucc29\/\uc751\uc9d1\ub825 \uc2e4\ud328\ub97c \uac10\uc9c0\ud560 \uc218 \uc788\uc2b5\ub2c8\ub2e4.<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-bbe0c25 elementor-reverse-mobile elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"bbe0c25\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-5bda47b\" data-id=\"5bda47b\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-353eff9 elementor-widget elementor-widget-heading\" data-id=\"353eff9\" data-element_type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\">\uce21\uc815 \ubaa9\ud45c<\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-5556e11 elementor-widget elementor-widget-text-editor\" data-id=\"5556e11\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p>\ubcf8 \uc5f0\uad6c\uc5d0\uc11c\ub294 NANOVEA\ub97c \uc18c\uac1c\ud569\ub2c8\ub2e4. <a href=\"https:\/\/nanovea.com\/tribometers\/\">\ud2b8\ub77c\uc774\ubcf4\ubbf8\ud130 <\/a>\uadf8\ub9ac\uace0 <a href=\"https:\/\/nanovea.com\/mechanical-testers\/\">\uae30\uacc4 \ud14c\uc2a4\ud130<\/a> \uc0b0\uc5c5\uc6a9 \ucf54\ud305\uc758 \ud3c9\uac00 \ubc0f \ud488\uc9c8 \uad00\ub9ac\uc5d0 \uc774\uc0c1\uc801\uc785\ub2c8\ub2e4.<\/p>\n<p>\ub2e4\uc591\ud55c \ud0d1\ucf54\ud2b8\uac00 \uc788\ub294 \uc544\ud06c\ub9b4 \uc6b0\ub808\ud0c4 \ubc14\ub2e5 \ud398\uc778\ud2b8\uc758 \ub9c8\ubaa8 \uacfc\uc815\uc740 \ub098\ub178\ubca0\uc544 \ud2b8\ub77c\uc774\ubcf4\ubbf8\ud130\ub97c \uc0ac\uc6a9\ud558\uc5ec \uc81c\uc5b4 \ubc0f \ubaa8\ub2c8\ud130\ub9c1 \ubc29\uc2dd\uc73c\ub85c \uc2dc\ubbac\ub808\uc774\uc158\ub429\ub2c8\ub2e4. \ub9c8\uc774\ud06c\ub85c \uc2a4\ud06c\ub798\uce58 \ud14c\uc2a4\ud2b8\ub294 \ud398\uc778\ud2b8\uc758 \uc751\uc9d1\ub825 \ub610\ub294 \uc811\ucc29\ub825 \uc2e4\ud328\ub97c \uc720\ubc1c\ud558\ub294 \ub370 \ud544\uc694\ud55c \ud558\uc911\uc744 \uce21\uc815\ud558\ub294 \ub370 \uc0ac\uc6a9\ub429\ub2c8\ub2e4.<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<section class=\"elementor-section elementor-inner-section elementor-element elementor-element-5986dd7 elementor-reverse-mobile elementor-section-full_width elementor-reverse-tablet elementor-section-height-default elementor-section-height-default\" data-id=\"5986dd7\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-extended\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-inner-column elementor-element elementor-element-a6b67e5\" data-id=\"a6b67e5\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-911a059 elementor-widget elementor-widget-image\" data-id=\"911a059\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<a href=\"https:\/\/nanovea.com\/instruments\/t100\/\">\n\t\t\t\t\t\t\t<img decoding=\"async\" width=\"763\" height=\"800\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2020\/12\/Nanovea-T100-Affordable-Tribometer.png\" class=\"elementor-animation-grow attachment-medium_large size-medium_large wp-image-9908\" alt=\"\uc18c\ud615 \uacf5\uc555 \ud2b8\ub77c\uc774\ubcf4\ubbf8\ud130 T100\" \/>\t\t\t\t\t\t\t\t<\/a>\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-cf30732 elementor-widget elementor-widget-text-editor\" data-id=\"cf30732\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<span style=\"color: #000000;\">\ub098\ub178\ube44\uc544 <\/span><span style=\"color: #1b96cf;\">T100<\/span>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-7429702 elementor-widget elementor-widget-text-editor\" data-id=\"7429702\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p style=\"text-align: center;\">\ucef4\ud329\ud2b8 \uacf5\uc555 \ud2b8\ub77c\uc774\ubcf4\ubbf8\ud130<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-48491b2 elementor-align-center learn-more-about-instrument elementor-widget elementor-widget-button\" data-id=\"48491b2\" data-element_type=\"widget\" data-widget_type=\"button.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<div class=\"elementor-button-wrapper\">\n\t\t\t\t\t<a class=\"elementor-button elementor-button-link elementor-size-md\" href=\"https:\/\/nanovea.com\/instruments\/t100\/\" id=\"learn-more-about-instrument\">\n\t\t\t\t\t\t<span class=\"elementor-button-content-wrapper\">\n\t\t\t\t\t\t\t\t\t<span class=\"elementor-button-text\">\uc790\uc138\ud788 \uc54c\uc544\ubcf4\uae30<\/span>\n\t\t\t\t\t<\/span>\n\t\t\t\t\t<\/a>\n\t\t\t\t<\/div>\n\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-inner-column elementor-element elementor-element-6a846d8\" data-id=\"6a846d8\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-3956283 elementor-widget elementor-widget-image\" data-id=\"3956283\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<a href=\"https:\/\/nanovea.com\/instruments\/pb1000\/\">\n\t\t\t\t\t\t\t<img decoding=\"async\" width=\"600\" height=\"595\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2022\/05\/NANOVEA-Mechanical-Tester-PB1000.png\" class=\"elementor-animation-grow attachment-medium_large size-medium_large wp-image-20051\" alt=\"\" \/>\t\t\t\t\t\t\t\t<\/a>\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-42860bf elementor-widget elementor-widget-text-editor\" data-id=\"42860bf\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p style=\"text-align: center;\"><span style=\"color: #000000;\">\ub098\ub178\ube44\uc544 <\/span><span style=\"color: #1b96cf;\">PB1000<\/span><\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-1f4a14e elementor-widget elementor-widget-text-editor\" data-id=\"1f4a14e\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p style=\"text-align: center;\">\ub300\ud615 \ud50c\ub7ab\ud3fc \uae30\uacc4 \ud14c\uc2a4\ud130<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-2c016cf elementor-align-center learn-more-about-instrument elementor-widget elementor-widget-button\" data-id=\"2c016cf\" data-element_type=\"widget\" data-widget_type=\"button.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<div class=\"elementor-button-wrapper\">\n\t\t\t\t\t<a class=\"elementor-button elementor-button-link elementor-size-md\" href=\"https:\/\/nanovea.com\/instruments\/pb1000\/\" id=\"learn-more-about-instrument\">\n\t\t\t\t\t\t<span class=\"elementor-button-content-wrapper\">\n\t\t\t\t\t\t\t\t\t<span class=\"elementor-button-text\">\uc790\uc138\ud788 \uc54c\uc544\ubcf4\uae30<\/span>\n\t\t\t\t\t<\/span>\n\t\t\t\t\t<\/a>\n\t\t\t\t<\/div>\n\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-1979bac elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"1979bac\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-no\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-c969083\" data-id=\"c969083\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-9c67049 elementor-widget elementor-widget-heading\" data-id=\"9c67049\" data-element_type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\">\ud14c\uc2a4\ud2b8 \uc808\ucc28<\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-1ad96b0 elementor-widget elementor-widget-text-editor\" data-id=\"1ad96b0\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p style=\"text-align: left;\">\uc774 \uc5f0\uad6c\uc5d0\uc11c\ub294 \ub0b4\uad6c\uc131\uc744 \ud5a5\uc0c1\uc2dc\ud0a4\uae30 \uc704\ud574 \ucca8\uac00\uc81c \ubc30\ud569\uc5d0 \uc57d\uac04\uc758 \ubcc0\ud654\ub97c \uc8fc\uba74\uc11c \ub3d9\uc77c\ud55c \ud504\ub77c\uc774\uba38(\ubca0\uc774\uc2a4 \ucf54\ud2b8)\uc640 \ub3d9\uc77c\ud55c \ud3ec\ubbac\ub7ec\uc758 \ub2e4\ub978 \ud0d1\ucf54\ud2b8\ub97c \uac00\uc9c4 \uc2dc\ud310\ub418\ub294 4\uac00\uc9c0 \uc218\uc131 \uc544\ud06c\ub9b4 \ubc14\ub2e5 \ucf54\ud305\uc81c\ub97c \ud3c9\uac00\ud569\ub2c8\ub2e4. \uc774 \ub124 \uac00\uc9c0 \ucf54\ud305\uc740 \uc0d8\ud50c A, B, C \ubc0f D\ub85c \uc2dd\ubcc4\ub429\ub2c8\ub2e4.<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-42252f7 elementor-widget elementor-widget-image\" data-id=\"42252f7\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img loading=\"lazy\" decoding=\"async\" width=\"1024\" height=\"436\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2022\/05\/Industrial-Paint-Tribology.jpg\" class=\"attachment-large size-large wp-image-20036\" alt=\"\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-3b1c09f elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"3b1c09f\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-top-column elementor-element elementor-element-c3e7d88\" data-id=\"c3e7d88\" data-element_type=\"column\" data-settings=\"{&quot;background_background&quot;:&quot;classic&quot;}\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-704243a elementor-widget elementor-widget-spacer\" data-id=\"704243a\" data-element_type=\"widget\" data-widget_type=\"spacer.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t<div class=\"elementor-spacer\">\n\t\t\t<div class=\"elementor-spacer-inner\"><\/div>\n\t\t<\/div>\n\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-top-column elementor-element elementor-element-f13c2c1\" data-id=\"f13c2c1\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-9e3708e elementor-widget elementor-widget-heading\" data-id=\"9e3708e\" data-element_type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\">\ucc29\uc6a9 \ud14c\uc2a4\ud2b8<\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-80398c0 elementor-widget elementor-widget-text-editor\" data-id=\"80398c0\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p style=\"text-align: left;\">NANOVEA \ub9c8\ucc30\uacc4\ub294 \ub9c8\ucc30\uacc4\uc218, COF, \ub0b4\ub9c8\ubaa8\uc131\uacfc \uac19\uc740 \ub9c8\ucc30\ud559\uc801 \uac70\ub3d9\uc744 \ud3c9\uac00\ud558\uae30 \uc704\ud574 \uc801\uc6a9\ub418\uc5c8\uc2b5\ub2c8\ub2e4. SS440 \ubcfc \ud301(\uc9c1\uacbd 6mm, \ub4f1\uae09 100)\uc744 \ud14c\uc2a4\ud2b8\ub41c \ud398\uc778\ud2b8\uc5d0 \uc801\uc6a9\ud588\uc2b5\ub2c8\ub2e4. COF\ub294 \ud604\uc7a5\uc5d0\uc11c \uae30\ub85d\ub418\uc5c8\uc2b5\ub2c8\ub2e4. \ub9c8\ubaa8\uc728 K\ub294 \uacf5\uc2dd K=V\/(F\u00d7s)=A\/(F\u00d7n)\uc744 \uc0ac\uc6a9\ud558\uc5ec \ud3c9\uac00\ub418\uc5c8\uc73c\uba70, \uc5ec\uae30\uc11c V\ub294 \ub9c8\ubaa8\ub7c9, F\ub294 \uc77c\ubc18 \ud558\uc911, s\ub294 \uc2ac\ub77c\uc774\ub529 \uac70\ub9ac, A\ub294 \ub9c8\ubaa8 \ud2b8\ub799\uc758 \ub2e8\uba74\uc801, n\uc740 \ud68c\uc804\uc218\uc785\ub2c8\ub2e4. \ud45c\uba74 \uac70\uce60\uae30\uc640 \ub9c8\ubaa8 \ud2b8\ub799 \ud504\ub85c\ud30c\uc77c\uc740 NANOVEA\uc5d0 \uc758\ud574 \ud3c9\uac00\ub418\uc5c8\uc2b5\ub2c8\ub2e4. <a href=\"https:\/\/nanovea.com\/profilometers\/\">\uad11\ud559 \ud504\ub85c\ud30c\uc77c\ub85c\ubbf8\ud130<\/a>, \ub9c8\ubaa8 \ud2b8\ub799 \ud615\ud0dc\ub294 \uad11\ud559 \ud604\ubbf8\uacbd\uc744 \uc0ac\uc6a9\ud558\uc5ec \uac80\uc0ac\ub418\uc5c8\uc2b5\ub2c8\ub2e4.<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-df053de elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"df053de\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-no\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-bbe3fd5\" data-id=\"bbe3fd5\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-0c30aad elementor-widget elementor-widget-heading\" data-id=\"0c30aad\" data-element_type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\">\ub9c8\ubaa8 \ud14c\uc2a4\ud2b8 \ub9e4\uac1c\ubcc0\uc218<\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<section class=\"elementor-section elementor-inner-section elementor-element elementor-element-a158972 elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"a158972\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-25 elementor-inner-column elementor-element elementor-element-a588777\" data-id=\"a588777\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap\">\n\t\t\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t<div class=\"elementor-column elementor-col-25 elementor-inner-column elementor-element elementor-element-d32c57a\" data-id=\"d32c57a\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-c0aad96 elementor-widget elementor-widget-text-editor\" data-id=\"c0aad96\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p>\uc77c\ubc18 \ud798<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-bafa675 elementor-widget elementor-widget-text-editor\" data-id=\"bafa675\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p>20 N<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t<div class=\"elementor-column elementor-col-25 elementor-inner-column elementor-element elementor-element-ce3ce36\" data-id=\"ce3ce36\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-3049f88 elementor-widget elementor-widget-text-editor\" data-id=\"3049f88\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p>\uc18d\ub3c4<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-a80a88a elementor-widget elementor-widget-text-editor\" data-id=\"a80a88a\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p>15m\/\ubd84<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t<div class=\"elementor-column elementor-col-25 elementor-inner-column elementor-element elementor-element-86350c3\" data-id=\"86350c3\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap\">\n\t\t\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<div class=\"elementor-element elementor-element-6bafc22 elementor-widget elementor-widget-text-editor\" data-id=\"6bafc22\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p>\ud14c\uc2a4\ud2b8 \uae30\uac04<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-8f4e1b9 elementor-widget elementor-widget-text-editor\" data-id=\"8f4e1b9\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p>100, 150, 300 \ubc0f 800 \uc0ac\uc774\ud074<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-575156f elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"575156f\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-top-column elementor-element elementor-element-a106cd2\" data-id=\"a106cd2\" data-element_type=\"column\" data-settings=\"{&quot;background_background&quot;:&quot;classic&quot;}\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-3aad899 elementor-widget elementor-widget-spacer\" data-id=\"3aad899\" data-element_type=\"widget\" data-widget_type=\"spacer.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t<div class=\"elementor-spacer\">\n\t\t\t<div class=\"elementor-spacer-inner\"><\/div>\n\t\t<\/div>\n\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-top-column elementor-element elementor-element-0387f33\" data-id=\"0387f33\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-1188445 elementor-widget elementor-widget-heading\" data-id=\"1188445\" data-element_type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\">\uc2a4\ud06c\ub798\uce58 \ud14c\uc2a4\ud2b8<\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-292fb67 elementor-widget elementor-widget-text-editor\" data-id=\"292fb67\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p style=\"text-align: left;\">\ub9c8\uc774\ud06c\ub85c \uc2a4\ud06c\ub798\uce58 \ud14c\uc2a4\ud130 \ubaa8\ub4dc\ub97c \uc0ac\uc6a9\ud558\uc5ec \ud398\uc778\ud2b8 \uc0d8\ud50c\uc5d0 \ub300\ud55c \uc810\uc9c4\uc801 \ud558\uc911 \uc2a4\ud06c\ub798\uce58 \ud14c\uc2a4\ud2b8\ub97c \uc218\ud589\ud558\uae30 \uc704\ud574 \ub85c\ud06c\uc6f0 C \ub2e4\uc774\uc544\ubaac\ub4dc \uc2a4\ud0c0\uc77c\ub7ec\uc2a4(\ubc18\uacbd 200\u03bcm)\uac00 \uc7a5\ucc29\ub41c \ub098\ub178\ubca0\uc544 \uae30\uacc4\uc2dd \ud14c\uc2a4\ud130\ub97c \uc0ac\uc6a9\ud588\uc2b5\ub2c8\ub2e4. \ub450 \uac00\uc9c0 \ucd5c\uc885 \ud558\uc911\uc774 \uc0ac\uc6a9\ub418\uc5c8\uc2b5\ub2c8\ub2e4: \ud504\ub77c\uc774\uba38\ub85c\ubd80\ud130 \ud398\uc778\ud2b8 \ubc15\ub9ac\ub97c \uc870\uc0ac\ud558\uae30 \uc704\ud55c \ucd5c\uc885 \ud558\uc911 5N\uacfc \uae08\uc18d \uae30\ud310\uc73c\ub85c\ubd80\ud130 \ud504\ub77c\uc774\uba38 \ubc15\ub9ac\ub97c \uc870\uc0ac\ud558\uae30 \uc704\ud55c \ucd5c\uc885 \ud558\uc911 35N\uc774 \uc0ac\uc6a9\ub418\uc5c8\uc2b5\ub2c8\ub2e4. \uacb0\uacfc\uc758 \uc7ac\ud604\uc131\uc744 \ubcf4\uc7a5\ud558\uae30 \uc704\ud574 \uac01 \uc0d8\ud50c\uc5d0 \ub300\ud574 \ub3d9\uc77c\ud55c \ud14c\uc2a4\ud2b8 \uc870\uac74\uc5d0\uc11c \uc138 \ubc88\uc758 \ud14c\uc2a4\ud2b8\ub97c \ubc18\ubcf5\ud588\uc2b5\ub2c8\ub2e4.<\/p><p style=\"text-align: left;\">\uc804\uccb4 \uc2a4\ud06c\ub798\uce58 \uae38\uc774\uc758 \ud30c\ub178\ub77c\ub9c8 \uc774\ubbf8\uc9c0\uac00 \uc790\ub3d9\uc73c\ub85c \uc0dd\uc131\ub418\uace0 \uc2dc\uc2a4\ud15c \uc18c\ud504\ud2b8\uc6e8\uc5b4\uc5d0 \uc758\ud574 \uc784\uacc4 \uace0\uc7a5 \uc704\uce58\uac00 \uc801\uc6a9\ub41c \ud558\uc911\uacfc \uc0c1\ud638 \uc5f0\uad00\ub418\uc5c8\uc2b5\ub2c8\ub2e4. \uc774 \uc18c\ud504\ud2b8\uc6e8\uc5b4 \uae30\ub2a5\uc744 \ud1b5\ud574 \uc0ac\uc6a9\uc790\ub294 \uc2a4\ud06c\ub798\uce58 \ud14c\uc2a4\ud2b8 \uc9c1\ud6c4 \ud604\ubbf8\uacbd\uc73c\ub85c \uc784\uacc4 \ud558\uc911\uc744 \uacb0\uc815\ud560 \ud544\uc694 \uc5c6\uc774 \uc5b8\uc81c\ub4e0\uc9c0 \uc2a4\ud06c\ub798\uce58 \ud2b8\ub799\uc5d0 \ub300\ud55c \ubd84\uc11d\uc744 \uc218\ud589\ud560 \uc218 \uc788\uc2b5\ub2c8\ub2e4.<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-4f2abf8 elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"4f2abf8\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-no\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-ef25143\" data-id=\"ef25143\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-09aead5 elementor-widget elementor-widget-heading\" data-id=\"09aead5\" data-element_type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\">\uc2a4\ud06c\ub798\uce58 \ud14c\uc2a4\ud2b8 \ub9e4\uac1c\ubcc0\uc218<\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-f48b766 elementor-widget elementor-widget-text-editor\" data-id=\"f48b766\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<table style=\"width: 100%;\"><tbody><tr><td style=\"text-align: left; width: 67.7419%;\"><em><strong>\ub85c\ub4dc \uc720\ud615<\/strong><\/em><\/td><td style=\"width: 29.912%; text-align: right;\"><em><strong>\ud504\ub85c\uadf8\ub808\uc2dc\ube0c<\/strong><\/em><\/td><\/tr><tr><td style=\"text-align: left; width: 67.7419%;\"><em><strong>\ucd08\uae30 \ub85c\ub4dc<\/strong><\/em><\/td><td style=\"width: 29.912%; text-align: right;\"><em><strong>0.01mN<\/strong><\/em><\/td><\/tr><tr><td style=\"text-align: left; width: 67.7419%;\"><em><strong>\ucd5c\uc885 \ub85c\ub4dc<\/strong><\/em><\/td><td style=\"width: 29.912%; text-align: right;\"><em><strong>5 N \/ 35 N<\/strong><\/em><\/td><\/tr><tr><td style=\"text-align: left; width: 67.7419%;\"><em><strong>\ub85c\ub529 \uc18d\ub3c4<\/strong><\/em><\/td><td style=\"width: 29.912%; text-align: right;\"><em><strong>10 \/ 70 N\/min<\/strong><\/em><\/td><\/tr><tr><td style=\"text-align: left; width: 67.7419%;\"><em><strong>\uc2a4\ud06c\ub798\uce58 \uae38\uc774<\/strong><\/em><\/td><td style=\"width: 29.912%; text-align: right;\"><em><strong>3mm<\/strong><\/em><\/td><\/tr><tr><td style=\"text-align: left; width: 67.7419%;\"><em><strong>\uc2a4\ud06c\ub798\uce6d \uc18d\ub3c4, dx\/dt<\/strong><\/em><\/td><td style=\"width: 29.912%; text-align: right;\"><em><strong>6.0mm\/\ubd84<\/strong><\/em><\/td><\/tr><tr><td style=\"text-align: left; width: 67.7419%;\"><em><strong>\ub4e4\uc5ec\uc4f0\uae30 \uae30\ud558\ud559<\/strong><\/em><\/td><td style=\"width: 29.912%; text-align: right;\"><em><strong>120\u00ba \ucf58<\/strong><\/em><\/td><\/tr><tr><td style=\"text-align: left; width: 67.7419%;\"><em><strong>\ub4e4\uc5ec\uc4f0\uae30 \uc7ac\ub8cc(\ud301)<\/strong><\/em><\/td><td style=\"width: 29.912%; text-align: right;\"><em><strong>\ub2e4\uc774\uc544\ubaac\ub4dc<\/strong><\/em><\/td><\/tr><tr><td style=\"text-align: left; width: 67.7419%;\"><em><strong>\ub4e4\uc5ec\uc4f0\uae30 \ud301 \ubc18\uacbd<\/strong><\/em><\/td><td style=\"width: 29.912%; text-align: right;\"><em><strong>200 \u03bcm<\/strong><\/em><\/td><\/tr><\/tbody><\/table>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-1fa8af8 elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"1fa8af8\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-no\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-5652dcb\" data-id=\"5652dcb\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-8896e58 elementor-widget elementor-widget-heading\" data-id=\"8896e58\" data-element_type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\">\ub9c8\ubaa8 \ud14c\uc2a4\ud2b8 \uacb0\uacfc<\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-9f3d908 elementor-widget elementor-widget-text-editor\" data-id=\"9f3d908\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p style=\"text-align: justify;\">\ub9c8\ubaa8 \ubcc0\ud654\ub97c \ubaa8\ub2c8\ud130\ub9c1\ud558\uae30 \uc704\ud574 \uac01 \uc0d8\ud50c\uc5d0 \ub300\ud574 \ub2e4\uc591\ud55c \ud68c\uc804 \uc218(100, 150, 300, 800 \uc0ac\uc774\ud074)\ub85c 4\ubc88\uc758 \ud540 \uc628 \ub514\uc2a4\ud06c \ub9c8\ubaa8 \ud14c\uc2a4\ud2b8\ub97c \uc218\ud589\ud588\uc2b5\ub2c8\ub2e4. \ub9c8\ubaa8 \ud14c\uc2a4\ud2b8\ub97c \uc218\ud589\ud558\uae30 \uc804\uc5d0 \ud45c\uba74 \uac70\uce60\uae30\ub97c \uc815\ub7c9\ud654\ud558\uae30 \uc704\ud574 \ub098\ub178\ubca0\uc544 3D \ube44\uc811\ucd09 \ud504\ub85c\ud30c\uc77c\ub7ec\ub85c \uc0d8\ud50c\uc758 \ud45c\uba74 \ud615\ud0dc\ub97c \uce21\uc815\ud588\uc2b5\ub2c8\ub2e4. \ubaa8\ub4e0 \uc0d8\ud50c\uc758 \ud45c\uba74 \uac70\uce60\uae30\ub294 \uadf8\ub9bc 1\uc5d0 \ud45c\uc2dc\ub41c \uac83\ucc98\ub7fc \uc57d 1\u03bcm\ub85c \ube44\uc2b7\ud588\uc2b5\ub2c8\ub2e4. \uadf8\ub9bc 2\uc640 \uac19\uc774 \ub9c8\ubaa8 \ud14c\uc2a4\ud2b8\uac00 \uc9c4\ud589\ub418\ub294 \ub3d9\uc548 COF\ub294 \ud604\uc7a5\uc5d0\uc11c \uae30\ub85d\ub418\uc5c8\uc2b5\ub2c8\ub2e4. \uadf8\ub9bc 4\ub294 100, 150, 300, 800 \uc0ac\uc774\ud074 \ud6c4 \ub9c8\ubaa8 \ud2b8\ub799\uc758 \ubcc0\ud654\ub97c \ubcf4\uc5ec\uc8fc\uba70, \uadf8\ub9bc 3\uc740 \ub9c8\ubaa8 \uacfc\uc815\uc758 \uc5ec\ub7ec \ub2e8\uacc4\uc5d0\uc11c \ub2e4\uc591\ud55c \uc0d8\ud50c\uc758 \ud3c9\uade0 \ub9c8\ubaa8\uc728\uc744 \uc694\uc57d\ud55c \uac83\uc785\ub2c8\ub2e4.<\/p><p>\u00a0<\/p><p style=\"text-align: justify;\">\ub2e4\ub978 \uc138 \uc0d8\ud50c\uc758 COF \uac12\uc774 ~0.07\uc778 \uac83\uacfc \ube44\uad50\ud558\uba74, \uc0d8\ud50c A\ub294 \ucc98\uc74c\uc5d0 ~0.15\ub85c \ud6e8\uc52c \ub192\uc740 COF\ub97c \ubcf4\uc774\ub2e4\uac00 \uc810\ucc28 \uc99d\uac00\ud558\uc5ec 300\ud68c \ub9c8\ubaa8 \uc0ac\uc774\ud074 \ud6c4 ~0.3\uc5d0\uc11c \uc548\uc815\ud654\ub429\ub2c8\ub2e4. \uc774\ub7ec\ud55c \ub192\uc740 COF\ub294 \ub9c8\ubaa8 \uacfc\uc815\uc744 \uac00\uc18d\ud654\ud558\uace0 \uadf8\ub9bc 4\uc5d0 \ud45c\uc2dc\ub41c \ubc14\uc640 \uac19\uc774 \uc0c1\ub2f9\ud55c \uc591\uc758 \ud398\uc778\ud2b8 \uc794\ud574\ub97c \uc0dd\uc131\ud569\ub2c8\ub2e4(\uc0d8\ud50c A\uc758 \ud0d1\ucf54\ud2b8\ub294 \ucc98\uc74c 100\ud68c \ud68c\uc804\uc5d0\uc11c \uc81c\uac70\ub418\uae30 \uc2dc\uc791\ud568). \uadf8\ub9bc 3\uc5d0\uc11c \ubcfc \uc218 \uc788\ub4ef\uc774, \uc0d8\ud50c A\ub294 \ucc98\uc74c 300\ud68c \ub3d9\uc548 ~5\u03bcm2\/N\uc758 \uac00\uc7a5 \ub192\uc740 \ub9c8\ubaa8\uc728\uc744 \ub098\ud0c0\ub0b4\uba70, \uae08\uc18d \uae30\ud310\uc758 \ub0b4\ub9c8\ubaa8\uc131\uc774 \ud5a5\uc0c1\ub418\uc5b4 ~3.5\u03bcm2\/N\uc73c\ub85c \uc57d\uac04 \uac10\uc18c\ud569\ub2c8\ub2e4. \uc0d8\ud50c C\uc758 \ud0d1\ucf54\ud2b8\ub294 \uadf8\ub9bc 4\uc5d0 \ud45c\uc2dc\ub41c \uac83\ucc98\ub7fc 150\ud68c \ub9c8\ubaa8 \uc0ac\uc774\ud074 \ud6c4\uc5d0 \uc2e4\ud328\ud558\uae30 \uc2dc\uc791\ud558\uba70, \uc774\ub294 \uadf8\ub9bc 2\uc5d0\uc11c COF\uc758 \uc99d\uac00\ub85c\ub3c4 \uc54c \uc218 \uc788\uc2b5\ub2c8\ub2e4.<\/p><p>\u00a0<\/p><p style=\"text-align: justify;\">\uc774\uc5d0 \ube44\ud574 \uc0d8\ud50c B\uc640 \uc0d8\ud50c D\ub294 \ud5a5\uc0c1\ub41c \ub9c8\ucc30 \ud2b9\uc131\uc744 \ubcf4\uc5ec\uc90d\ub2c8\ub2e4. \uc0d8\ud50c B\ub294 \uc804\uccb4 \ud14c\uc2a4\ud2b8 \uae30\uac04 \ub3d9\uc548 \ub0ae\uc740 COF\ub97c \uc720\uc9c0\ud558\uba70, COF\uac00 ~0.05\uc5d0\uc11c ~0.1\ub85c \uc57d\uac04 \uc99d\uac00\ud569\ub2c8\ub2e4. \uc774\ub7ec\ud55c \uc724\ud65c \ud6a8\uacfc\ub294 \ub0b4\ub9c8\ubaa8\uc131\uc744 \ud06c\uac8c \ud5a5\uc0c1\uc2dc\ucf1c 800\ud68c \ub9c8\ubaa8 \uc0ac\uc774\ud074 \ud6c4\uc5d0\ub3c4 \ud0d1\ucf54\ud2b8\uac00 \uc5ec\uc804\ud788 \ubc11\uc5d0 \uc788\ub294 \ud504\ub77c\uc774\uba38\uc5d0 \uc6b0\uc218\ud55c \ubcf4\ud638 \uae30\ub2a5\uc744 \uc81c\uacf5\ud569\ub2c8\ub2e4. 800 \uc0ac\uc774\ud074\uc5d0\uc11c \uc0d8\ud50c B\uc758 \ud3c9\uade0 \ub9c8\ubaa8\uc728\uc740 ~0.77 \u03bcm2\/N\uc5d0 \ubd88\uacfc\ud55c \ucd5c\uc800\uce58\ub97c \uae30\ub85d\ud588\uc2b5\ub2c8\ub2e4. \uc0d8\ud50c D\uc758 \ud0d1\ucf54\ud2b8\ub294 375 \uc0ac\uc774\ud074 \ud6c4\uc5d0 \ubc15\ub9ac\ub418\uae30 \uc2dc\uc791\ud558\ub294\ub370, \uc774\ub294 \uadf8\ub9bc 2\uc758 \uac11\uc791\uc2a4\ub7ec\uc6b4 COF \uc99d\uac00\uc5d0 \ubc18\uc601\ub418\uc5b4 \uc788\uc2b5\ub2c8\ub2e4. \uc0d8\ud50c D\uc758 \ud3c9\uade0 \ub9c8\ubaa8\uc728\uc740 800 \uc0ac\uc774\ud074\uc5d0\uc11c ~1.1 \u03bcm2\/N\uc785\ub2c8\ub2e4.<\/p><p>\u00a0<\/p><p style=\"text-align: justify;\">\uae30\uc874\uc758 \ud14c\uc774\ubc84 \ub9c8\ubaa8 \uce21\uc815\uacfc \ube44\uad50\ud558\uc5ec \ub098\ub178\ubca0\uc544 \ud2b8\ub77c\uc774\ubcf4\ubbf8\ud130\ub294 \uc0c1\uc5c5\uc6a9 \ubc14\ub2e5\/\uc790\ub3d9\ucc28 \ud398\uc778\ud2b8\uc758 \uc7ac\ud604 \uac00\ub2a5\ud55c \ud3c9\uac00 \ubc0f \ud488\uc9c8 \uad00\ub9ac\ub97c \ubcf4\uc7a5\ud558\ub294 \uc798 \uc81c\uc5b4\ub418\uace0 \uc815\ub7c9\ud654\ub418\uace0 \uc2e0\ub8b0\ud560 \uc218 \uc788\ub294 \ub9c8\ubaa8 \ud3c9\uac00\ub97c \uc81c\uacf5\ud569\ub2c8\ub2e4. \ub610\ud55c, \ud604\uc7a5 COF \uce21\uc815 \uae30\ub2a5\uc744 \ud1b5\ud574 \uc0ac\uc6a9\uc790\ub294 \ub9c8\ubaa8 \uacf5\uc815\uc758 \uc5ec\ub7ec \ub2e8\uacc4\ub97c COF\uc758 \ubcc0\ud654\uc640 \uc5f0\uad00\uc2dc\ud0ac \uc218 \uc788\uc73c\uba70, \uc774\ub294 \ub2e4\uc591\ud55c \ud398\uc778\ud2b8 \ucf54\ud305\uc758 \ub9c8\ubaa8 \uba54\ucee4\ub2c8\uc998 \ubc0f \ub9c8\ucc30 \ud2b9\uc131\uc5d0 \ub300\ud55c \uadfc\ubcf8\uc801\uc778 \uc774\ud574\ub97c \ud5a5\uc0c1\uc2dc\ud0a4\ub294 \ub370 \ub9e4\uc6b0 \uc911\uc694\ud569\ub2c8\ub2e4.<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-7311885 elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"7311885\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-b11fd5d\" data-id=\"b11fd5d\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<section class=\"elementor-section elementor-inner-section elementor-element elementor-element-f59c5b1 elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"f59c5b1\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-inner-column elementor-element elementor-element-7a5dc99\" data-id=\"7a5dc99\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-40fab7c elementor-widget elementor-widget-image\" data-id=\"40fab7c\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img loading=\"lazy\" decoding=\"async\" width=\"366\" height=\"345\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2022\/05\/Industrial-Coatings-Profilometry.jpg\" class=\"attachment-large size-large wp-image-20026\" alt=\"\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-inner-column elementor-element elementor-element-24174e9\" data-id=\"24174e9\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-964c701 elementor-widget elementor-widget-image\" data-id=\"964c701\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img loading=\"lazy\" decoding=\"async\" width=\"366\" height=\"345\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2022\/05\/Industrial-Coatings-Roughness.jpg\" class=\"attachment-large size-large wp-image-20027\" alt=\"\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-inner-section elementor-element elementor-element-feddc4b elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"feddc4b\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-inner-column elementor-element elementor-element-3bed450\" data-id=\"3bed450\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-58312f2 elementor-widget elementor-widget-image\" data-id=\"58312f2\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img loading=\"lazy\" decoding=\"async\" width=\"366\" height=\"345\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2022\/05\/Industrial-Paint-Roughness.jpg\" class=\"attachment-large size-large wp-image-20031\" alt=\"\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-inner-column elementor-element elementor-element-2a63829\" data-id=\"2a63829\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-641c302 elementor-widget elementor-widget-image\" data-id=\"641c302\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img loading=\"lazy\" decoding=\"async\" width=\"366\" height=\"345\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2022\/05\/Industrial-Paint-Testing.jpg\" class=\"attachment-large size-large wp-image-20035\" alt=\"\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<div class=\"elementor-element elementor-element-4103861 elementor-widget elementor-widget-text-editor\" data-id=\"4103861\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p style=\"text-align: center;\"><span class=\"fontstyle0\" style=\"color: #1b96cf;\">\uadf8\ub9bc 1: <\/span><span class=\"fontstyle0\" style=\"color: #1b96cf;\"><span style=\"color: #000000;\"><span class=\"fontstyle0\">\ud398\uc778\ud2b8 \uc0d8\ud50c\uc758 3D \ud615\ud0dc \ubc0f \uac70\uce60\uae30.<\/span>\n<\/span><\/span><\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<section class=\"elementor-section elementor-inner-section elementor-element elementor-element-eea6b5a elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"eea6b5a\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-inner-column elementor-element elementor-element-7e36f39\" data-id=\"7e36f39\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-868b4e2 elementor-widget elementor-widget-image\" data-id=\"868b4e2\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img loading=\"lazy\" decoding=\"async\" width=\"719\" height=\"508\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2022\/05\/Industrial-Coatings-COF.jpg\" class=\"attachment-large size-large wp-image-20024\" alt=\"\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-0cfdbaa elementor-widget elementor-widget-text-editor\" data-id=\"0cfdbaa\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p style=\"text-align: center;\"><span class=\"fontstyle0\" style=\"color: #1b96cf;\">\uadf8\ub9bc 2: <\/span><span style=\"color: #000000;\"><span class=\"fontstyle0\">\ud540 \uc628 \ub514\uc2a4\ud06c \ud14c\uc2a4\ud2b8 \uc911 COF.<\/span><\/span><\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-inner-column elementor-element elementor-element-5864534\" data-id=\"5864534\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-9ee2592 elementor-widget elementor-widget-image\" data-id=\"9ee2592\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img loading=\"lazy\" decoding=\"async\" width=\"719\" height=\"508\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2022\/05\/Industrial-Coating-Wear-Test.jpg\" class=\"attachment-large size-large wp-image-20023\" alt=\"\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-6f42a0a elementor-widget elementor-widget-text-editor\" data-id=\"6f42a0a\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p style=\"text-align: center;\"><span class=\"fontstyle0\" style=\"color: #1b96cf;\">\uadf8\ub9bc 3: <\/span><span style=\"color: #000000;\"><span class=\"fontstyle0\">\ub2e4\uc591\ud55c \ud398\uc778\ud2b8\uc758 \ub9c8\ubaa8\uc728\uc758 \uc9c4\ud654.<\/span><\/span><\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<div class=\"elementor-element elementor-element-4015260 elementor-widget elementor-widget-image\" data-id=\"4015260\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img loading=\"lazy\" decoding=\"async\" width=\"1024\" height=\"801\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2022\/05\/Industrial-Paint-Wear-Test.jpg\" class=\"attachment-large size-large wp-image-20037\" alt=\"\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-56e7fda elementor-widget elementor-widget-text-editor\" data-id=\"56e7fda\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p style=\"text-align: center;\"><span class=\"fontstyle0\" style=\"color: #1b96cf;\">\uadf8\ub9bc 4: <\/span><span class=\"fontstyle0\" style=\"color: #1b96cf;\"><span style=\"color: #000000;\"><span class=\"fontstyle0\">\ud540 \uc628 \ub514\uc2a4\ud06c \ud14c\uc2a4\ud2b8 \uc911 \ub9c8\ubaa8 \ud2b8\ub799\uc758 \uc9c4\ud654.<\/span>\n<\/span><\/span><\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-ec03633 elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"ec03633\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-no\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-c910bc7\" data-id=\"c910bc7\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-99fcb17 elementor-widget elementor-widget-heading\" data-id=\"99fcb17\" data-element_type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\">\uc2a4\ud06c\ub798\uce58 \ud14c\uc2a4\ud2b8 \uacb0\uacfc<\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-4398642 elementor-widget elementor-widget-text-editor\" data-id=\"4398642\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p style=\"text-align: justify;\">\uadf8\ub9bc 5\ub294 \uc0d8\ud50c A\uc758 \uc2a4\ud06c\ub798\uce58 \uae38\uc774\uc5d0 \ub530\ub978 \uc815\uc0c1 \ud798, \ub9c8\ucc30\ub825 \ubc0f \uc2e4\uc81c \uae4a\uc774\uc758 \ud50c\ub86f\uc744 \uc608\ub85c \ub4e4\uc5b4 \ubcf4\uc5ec\uc90d\ub2c8\ub2e4. \uc635\uc158\uc73c\ub85c \uc81c\uacf5\ub418\ub294 \uc74c\ud5a5 \ubc29\ucd9c \ubaa8\ub4c8\uc744 \uc124\uce58\ud558\uba74 \ub354 \ub9ce\uc740 \uc815\ubcf4\ub97c \uc5bb\uc744 \uc218 \uc788\uc2b5\ub2c8\ub2e4. \uc815\uc0c1 \ud558\uc911\uc774 \uc120\ud615\uc801\uc73c\ub85c \uc99d\uac00\ud568\uc5d0 \ub530\ub77c \uc555\ud754 \ud301\uc740 \uc2e4\uc81c \uae4a\uc774\uc758 \uc810\uc9c4\uc801\uc778 \uc99d\uac00\uc5d0 \ubc18\uc601\ub418\uc5b4 \ud14c\uc2a4\ud2b8 \uc0d8\ud50c\uc5d0 \uc810\ucc28\uc801\uc73c\ub85c \uac00\ub77c \uc549\uc2b5\ub2c8\ub2e4. \ub9c8\ucc30\ub825 \ubc0f \uc2e4\uc81c \uae4a\uc774 \uace1\uc120\uc758 \uae30\uc6b8\uae30 \ubcc0\ud654\ub294 \ucf54\ud305 \uc2e4\ud328\uac00 \ubc1c\uc0dd\ud558\uae30 \uc2dc\uc791\ud55c\ub2e4\ub294 \uc758\ubbf8 \uc911 \ud558\ub098\ub85c \uc0ac\uc6a9\ud560 \uc218 \uc788\uc2b5\ub2c8\ub2e4.<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-fe155f9 elementor-widget elementor-widget-image\" data-id=\"fe155f9\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img loading=\"lazy\" decoding=\"async\" width=\"926\" height=\"495\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2022\/05\/Industrial-Coating-Scratch-Test.jpg\" class=\"attachment-large size-large wp-image-20044\" alt=\"\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-43838d4 elementor-widget elementor-widget-text-editor\" data-id=\"43838d4\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p style=\"text-align: center;\"><span class=\"fontstyle0\" style=\"color: #1b96cf;\">\uadf8\ub9bc 5: <\/span><span class=\"fontstyle0\" style=\"color: #1b96cf;\"><span style=\"color: #000000;\"><span class=\"fontstyle0\">\uc2a4\ud06c\ub798\uce58 \uae38\uc774\uc758 \ud568\uc218\ub85c\uc11c\uc758 \uc815\uc0c1 \ud798, \ub9c8\ucc30\ub825 \ubc0f \uc2e4\uc81c \uae4a\uc774\n\ucd5c\ub300 \ud558\uc911\uc774 5N\uc778 \uc0d8\ud50c A\uc758 \uc2a4\ud06c\ub798\uce58 \ud14c\uc2a4\ud2b8.<\/span>\n<\/span><\/span><\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-4762328 elementor-widget elementor-widget-text-editor\" data-id=\"4762328\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p style=\"text-align: justify;\">\uadf8\ub9bc 6\uacfc \uadf8\ub9bc 7\uc740 \uac01\uac01 \ucd5c\ub300 \ud558\uc911 5N\uacfc 35N\uc73c\ub85c \ud14c\uc2a4\ud2b8\ud55c \ub124 \uac00\uc9c0 \ud398\uc778\ud2b8 \uc0d8\ud50c \ubaa8\ub450\uc758 \uc804\uccb4 \uc2a4\ud06c\ub798\uce58\ub97c \ubcf4\uc5ec\uc90d\ub2c8\ub2e4. \uc0d8\ud50c D\ub294 \ud504\ub77c\uc774\uba38\ub97c \ubc15\ub9ac\ud558\uae30 \uc704\ud574 50N\uc758 \ub354 \ub192\uc740 \ud558\uc911\uc774 \ud544\uc694\ud588\uc2b5\ub2c8\ub2e4. 5N \ucd5c\uc885 \ud558\uc911\uc5d0\uc11c\uc758 \uc2a4\ud06c\ub798\uce58 \ud14c\uc2a4\ud2b8(\uadf8\ub9bc 6)\ub294 \uc0c1\ub2e8 \ud398\uc778\ud2b8\uc758 \uc751\uc9d1\ub825\/\uc811\ucc29\ub825 \uc2e4\ud328\ub97c \ud3c9\uac00\ud558\uace0, 35N\uc5d0\uc11c\uc758 \ud14c\uc2a4\ud2b8(\uadf8\ub9bc 7)\ub294 \ud504\ub77c\uc774\uba38\uc758 \ubc15\ub9ac\ub97c \ud3c9\uac00\ud569\ub2c8\ub2e4. \ud604\ubbf8\uacbd \uc0ac\uc9c4\uc758 \ud654\uc0b4\ud45c\ub294 \uc0c1\ub2e8 \ucf54\ud305 \ub610\ub294 \ud504\ub77c\uc774\uba38\uac00 \ud504\ub77c\uc774\uba38 \ub610\ub294 \uae30\ud310\uc5d0\uc11c \uc644\uc804\ud788 \uc81c\uac70\ub418\uae30 \uc2dc\uc791\ud558\ub294 \uc9c0\uc810\uc744 \ub098\ud0c0\ub0c5\ub2c8\ub2e4. \uc774 \uc2dc\uc810\uc758 \ud558\uc911\uc744 \uc784\uacc4 \ud558\uc911(Lc)\uc774\ub77c\uace0 \ud558\uba70, \ud45c 1\uc5d0 \uc694\uc57d\ub41c \ub300\ub85c \ud398\uc778\ud2b8\uc758 \uc751\uc9d1\ub825 \ub610\ub294 \uc811\ucc29 \ud2b9\uc131\uc744 \ube44\uad50\ud558\ub294 \ub370 \uc0ac\uc6a9\ub429\ub2c8\ub2e4.<\/p><p style=\"text-align: justify;\">\u00a0<\/p><p style=\"text-align: justify;\">\ud398\uc778\ud2b8 \ubc15\ub9ac \uc2dc 4.04N, \ud504\ub77c\uc774\uba38 \ubc15\ub9ac \uc2dc 36.61N\uc758 \uac00\uc7a5 \ub192\uc740 Lc \uac12\uc744 \ub098\ud0c0\ub0b4\ub294 \ud398\uc778\ud2b8 \uc0d8\ud50c D\uac00 \uacc4\uba74 \uc811\ucc29\ub825\uc774 \uac00\uc7a5 \uc6b0\uc218\ud558\ub2e4\ub294 \uac83\uc774 \ubd84\uba85\ud569\ub2c8\ub2e4. \uc0d8\ud50c B\ub294 \ub450 \ubc88\uc9f8\ub85c \uc6b0\uc218\ud55c \uc2a4\ud06c\ub798\uce58 \uc800\ud56d\uc131\uc744 \ubcf4\uc5ec\uc90d\ub2c8\ub2e4. \uc2a4\ud06c\ub798\uce58 \ubd84\uc11d \uacb0\uacfc, \ud398\uc778\ud2b8 \ud3ec\ubbac\ub7ec\uc758 \ucd5c\uc801\ud654\uac00 \uc544\ud06c\ub9b4 \ubc14\ub2e5 \ud398\uc778\ud2b8\uc758 \uae30\uacc4\uc801 \uac70\ub3d9, \ub354 \uad6c\uccb4\uc801\uc73c\ub85c\ub294 \uc2a4\ud06c\ub798\uce58 \uc800\ud56d\uc131\uacfc \uc811\ucc29 \ud2b9\uc131\uc5d0 \ub9e4\uc6b0 \uc911\uc694\ud558\ub2e4\ub294 \uac83\uc744 \uc54c \uc218 \uc788\uc2b5\ub2c8\ub2e4.<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-214f524 elementor-widget elementor-widget-image\" data-id=\"214f524\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img loading=\"lazy\" decoding=\"async\" width=\"1024\" height=\"225\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2022\/05\/Industrial-Paint-QC.jpg\" class=\"attachment-large size-large wp-image-20030\" alt=\"\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-a992b7a elementor-widget elementor-widget-text-editor\" data-id=\"a992b7a\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p style=\"text-align: center;\"><span class=\"fontstyle0\" style=\"color: #1b96cf;\">\ud45c 1: <\/span><span class=\"fontstyle0\" style=\"color: #1b96cf;\"><span style=\"color: #000000;\"><span class=\"fontstyle0\">\uc784\uacc4 \ubd80\ud558 \uc694\uc57d.<\/span>\n<\/span><\/span><\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-39ae57e elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"39ae57e\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-20028cc\" data-id=\"20028cc\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-762a9a3 elementor-widget elementor-widget-image\" data-id=\"762a9a3\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img loading=\"lazy\" decoding=\"async\" width=\"1024\" height=\"196\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2022\/05\/Industrial-Coating-Scratch.jpg\" class=\"attachment-large size-large wp-image-20042\" alt=\"\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-6e5aa76 elementor-widget elementor-widget-image\" data-id=\"6e5aa76\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img loading=\"lazy\" decoding=\"async\" width=\"1024\" height=\"198\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2022\/05\/Industrial-Coating-Scratch-Testing.jpg\" class=\"attachment-large size-large wp-image-20041\" alt=\"\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-e9a0a91 elementor-widget elementor-widget-image\" data-id=\"e9a0a91\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img loading=\"lazy\" decoding=\"async\" width=\"1024\" height=\"198\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2022\/05\/Industrial-Coating-Scratch-Tester.jpg\" class=\"attachment-large size-large wp-image-20040\" alt=\"\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-ef0ba5a elementor-widget elementor-widget-image\" data-id=\"ef0ba5a\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img loading=\"lazy\" decoding=\"async\" width=\"1024\" height=\"198\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2022\/05\/Industrial-Coating-Scratch-QC-Test.jpg\" class=\"attachment-large size-large wp-image-20039\" alt=\"\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-b136a8f elementor-widget elementor-widget-text-editor\" data-id=\"b136a8f\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p style=\"text-align: center;\"><span class=\"fontstyle0\" style=\"color: #1b96cf;\">\uadf8\ub9bc 6: <\/span><span class=\"fontstyle0\" style=\"color: #1b96cf;\"><span style=\"color: #000000;\"><span class=\"fontstyle0\">\ucd5c\ub300 \ud558\uc911 5N\uc758 \uc804\uccb4 \uc2a4\ud06c\ub798\uce58 \ud604\ubbf8\uacbd \uc0ac\uc9c4.<\/span>\n<\/span><\/span><\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-3dd028d elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"3dd028d\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-36cb163\" data-id=\"36cb163\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-d35b065 elementor-widget elementor-widget-image\" data-id=\"d35b065\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img loading=\"lazy\" decoding=\"async\" width=\"1024\" height=\"198\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2022\/05\/Industrial-Paint-Scratch-Test.jpg\" class=\"attachment-large size-large wp-image-20033\" alt=\"\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-daf897a elementor-widget elementor-widget-image\" data-id=\"daf897a\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img loading=\"lazy\" decoding=\"async\" width=\"1024\" height=\"198\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2022\/05\/Industrial-Paint-Scratch-Testing.jpg\" class=\"attachment-large size-large wp-image-20034\" alt=\"\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-20c9e99 elementor-widget elementor-widget-image\" data-id=\"20c9e99\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img loading=\"lazy\" decoding=\"async\" width=\"1024\" height=\"198\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2022\/05\/Industrial-Paint-Lab-Testing.jpg\" class=\"attachment-large size-large wp-image-20029\" alt=\"\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-f7b4a00 elementor-widget elementor-widget-image\" data-id=\"f7b4a00\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img loading=\"lazy\" decoding=\"async\" width=\"1024\" height=\"148\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2022\/05\/Industrial-Paint-Scratch-QC-Test.jpg\" class=\"attachment-large size-large wp-image-20032\" alt=\"\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-9a86977 elementor-widget elementor-widget-text-editor\" data-id=\"9a86977\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p style=\"text-align: center;\"><span class=\"fontstyle0\" style=\"color: #1b96cf;\">\uadf8\ub9bc 7: <\/span><span class=\"fontstyle0\" style=\"color: #1b96cf;\"><span style=\"color: #000000;\"><span class=\"fontstyle0\">\ucd5c\ub300 \ud558\uc911 35N\uc758 \uc804\uccb4 \uc2a4\ud06c\ub798\uce58 \ud604\ubbf8\uacbd \uc0ac\uc9c4.<\/span>\n<\/span><\/span><\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-c8c9bdf elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"c8c9bdf\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-724e51f\" data-id=\"724e51f\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-ec6977f elementor-widget elementor-widget-heading\" data-id=\"ec6977f\" data-element_type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\">\uacb0\ub860<\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-dcde8ed elementor-widget elementor-widget-text-editor\" data-id=\"dcde8ed\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p style=\"text-align: justify;\">\uae30\uc874\uc758 \ud14c\uc774\ubc84 \ub9c8\ubaa8 \uce21\uc815\uacfc \ube44\uad50\ud588\uc744 \ub54c, \ub098\ub178\ubca0\uc544 \uba54\uce74\ub2c8\uceec \ud14c\uc2a4\ud130\uc640 \ud2b8\ub77c\uc774\ubcf4\ubbf8\ud130\ub294 \uc0c1\uc5c5\uc6a9 \ubc14\ub2e5 \ubc0f \uc790\ub3d9\ucc28 \ucf54\ud305\uc758 \ud3c9\uac00 \ubc0f \ud488\uc9c8 \uad00\ub9ac\ub97c \uc704\ud55c \ud0c1\uc6d4\ud55c \ub3c4\uad6c\uc785\ub2c8\ub2e4. \uc2a4\ud06c\ub798\uce58 \ubaa8\ub4dc\uc758 \ub098\ub178\ubca0\uc544 \uba54\uce74\ub2c8\uceec \ud14c\uc2a4\ud130\ub294 \ucf54\ud305 \uc2dc\uc2a4\ud15c\uc758 \uc811\ucc29\/\uc751\uc9d1\ub825 \ubb38\uc81c\ub97c \uac10\uc9c0\ud560 \uc218 \uc788\uc2b5\ub2c8\ub2e4. \ub098\ub178\ubca0\uc544 \ud2b8\ub77c\uc774\ubcf4\ubbf8\ud130\ub294 \ud398\uc778\ud2b8\uc758 \ub0b4\ub9c8\ubaa8\uc131 \ubc0f \ub9c8\ucc30 \uacc4\uc218\uc5d0 \ub300\ud574 \uc798 \uc81c\uc5b4\ub418\uace0 \uc815\ub7c9\ud654 \ubc0f \ubc18\ubcf5 \uac00\ub2a5\ud55c \ub9c8\ucc30\ud559\uc801 \ubd84\uc11d\uc744 \uc81c\uacf5\ud569\ub2c8\ub2e4.<\/p><p>\u00a0<\/p><p>\uc774 \uc5f0\uad6c\uc5d0\uc11c \ud14c\uc2a4\ud2b8\ud55c \uc218\uc131 \uc544\ud06c\ub9b4 \ubc14\ub2e5 \ucf54\ud305\uc5d0 \ub300\ud55c \uc885\ud569\uc801\uc778 \ub9c8\ucc30 \ubc0f \uae30\uacc4\uc801 \ubd84\uc11d\uc5d0 \ub530\ub974\uba74, \uc0d8\ud50c B\uac00 \uac00\uc7a5 \ub0ae\uc740 COF \ubc0f \ub9c8\ubaa8\uc728\uacfc \ub450 \ubc88\uc9f8\ub85c \uc6b0\uc218\ud55c \uc2a4\ud06c\ub798\uce58 \uc800\ud56d\uc131\uc744 \ubcf4\uc600\uc73c\uba70, \uc0d8\ud50c D\ub294 \uac00\uc7a5 \uc6b0\uc218\ud55c \uc2a4\ud06c\ub798\uce58 \uc800\ud56d\uc131\uacfc \ub450 \ubc88\uc9f8\ub85c \uc6b0\uc218\ud55c \ub0b4\ub9c8\ubaa8\uc131\uc744 \ub098\ud0c0\ub0c8\uc2b5\ub2c8\ub2e4. \uc774 \ud3c9\uac00\ub97c \ud1b5\ud574 \ub2e4\uc591\ud55c \uc801\uc6a9 \ud658\uacbd\uc758 \uc694\uad6c \uc0ac\ud56d\uc5d0 \ub9de\ub294 \ucd5c\uc801\uc758 \ud6c4\ubcf4\ub97c \ud3c9\uac00\ud558\uace0 \uc120\ud0dd\ud560 \uc218 \uc788\uc2b5\ub2c8\ub2e4.<\/p><p>\u00a0<\/p><p>\ub098\ub178\ubca0\uc544 \uae30\uacc4\uc2dd \uc2dc\ud5d8\uae30\uc758 \ub098\ub178 \ubc0f \ub9c8\uc774\ud06c\ub85c \ubaa8\ub4c8\uc740 \ubaa8\ub450 ISO \ubc0f ASTM\uc744 \uc900\uc218\ud558\ub294 \uc555\ud754, \uc2a4\ud06c\ub798\uce58 \ubc0f \ub9c8\ubaa8 \uc2dc\ud5d8\uae30 \ubaa8\ub4dc\ub97c \ud3ec\ud568\ud558\uace0 \uc788\uc5b4 \ub2e8\uc77c \ubaa8\ub4c8\uc5d0\uc11c \ud398\uc778\ud2b8 \ud3c9\uac00\uc5d0 \uc0ac\uc6a9\ud560 \uc218 \uc788\ub294 \uac00\uc7a5 \uad11\ubc94\uc704\ud55c \ud14c\uc2a4\ud2b8\ub97c \uc81c\uacf5\ud569\ub2c8\ub2e4. \ub098\ub178\ubca0\uc544 \ud2b8\ub77c\uc774\ubcf4\ubbf8\ud130\ub294 ISO \ubc0f ASTM\uc744 \uc900\uc218\ud558\ub294 \ud68c\uc804 \ubc0f \uc120\ud615 \ubaa8\ub4dc\ub97c \uc0ac\uc6a9\ud558\uc5ec \uc815\ubc00\ud558\uace0 \ubc18\ubcf5 \uac00\ub2a5\ud55c \ub9c8\ubaa8 \ubc0f \ub9c8\ucc30 \ud14c\uc2a4\ud2b8\ub97c \uc81c\uacf5\ud558\uba70, \ud558\ub098\uc758 \uc0ac\uc804 \ud1b5\ud569\ub41c \uc2dc\uc2a4\ud15c\uc5d0\uc11c \uace0\uc628 \ub9c8\ubaa8, \uc724\ud65c \ubc0f \ud2b8\ub9ac\ubcf4 \ubd80\uc2dd \ubaa8\ub4c8\uc744 \uc635\uc158\uc73c\ub85c \uc0ac\uc6a9\ud560 \uc218 \uc788\uc2b5\ub2c8\ub2e4. \ub098\ub178\ubca0\uc544\uc758 \ud0c1\uc6d4\ud55c \uc81c\ud488\uad70\uc740 \uacbd\ub3c4, \uc601 \uacc4\uc218, \ud30c\uad34 \uc778\uc131, \uc811\ucc29\ub825, \ub0b4\ub9c8\ubaa8\uc131 \ub4f1 \uc587\uac70\ub098 \ub450\uaebc\uc6b4, \uc5f0\uc9c8 \ub610\ub294 \uacbd\uc9c8 \ucf54\ud305, \ud544\ub984 \ubc0f \uae30\ud310\uc758 \ubaa8\ub4e0 \uae30\uacc4\uc801\/ \ub9c8\ucc30\ud559\uc801 \ud2b9\uc131\uc744 \uce21\uc815\ud558\ub294 \ub370 \uc774\uc0c1\uc801\uc778 \uc194\ub8e8\uc158\uc785\ub2c8\ub2e4. \uc635\uc158\uc73c\ub85c \uc81c\uacf5\ub418\ub294 \ub098\ub178\ubca0\uc544 \ube44\uc811\ucd09\uc2dd \uad11\ud559 \ud504\ub85c\ud30c\uc77c\ub7ec\ub294 \uac70\uce60\uae30\uc640 \uac19\uc740 \uae30\ud0c0 \ud45c\uba74 \uce21\uc815 \uc678\uc5d0\ub3c4 \uc2a4\ud06c\ub798\uce58 \ubc0f \ub9c8\ubaa8 \ud2b8\ub799\uc758 \uace0\ud574\uc0c1\ub3c4 3D \uc774\ubbf8\uc9d5\uc744 \uc704\ud574 \uc0ac\uc6a9\ud560 \uc218 \uc788\uc2b5\ub2c8\ub2e4.<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-e71b01c elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"e71b01c\" data-element_type=\"section\" data-settings=\"{&quot;background_background&quot;:&quot;classic&quot;}\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-4393a2f\" data-id=\"4393a2f\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-53db75e elementor-widget elementor-widget-heading\" data-id=\"53db75e\" data-element_type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\"><b>\uc774\uc81c \uc560\ud50c\ub9ac\ucf00\uc774\uc158\uc5d0 \ub300\ud574 \uc774\uc57c\uae30\ud574 \ubcf4\uaca0\uc2b5\ub2c8\ub2e4.<\/b><\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-d73f295 live-chat elementor-align-center elementor-widget elementor-widget-button\" data-id=\"d73f295\" data-element_type=\"widget\" data-widget_type=\"button.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<div class=\"elementor-button-wrapper\">\n\t\t\t\t\t<a class=\"elementor-button elementor-button-link elementor-size-md\" href=\"https:\/\/nanovea.com\/contact\/live-chat\/\" id=\"live-chat\">\n\t\t\t\t\t\t<span class=\"elementor-button-content-wrapper\">\n\t\t\t\t\t\t\t\t\t<span class=\"elementor-button-text\">\ub77c\uc774\ube0c \ucc44\ud305<\/span>\n\t\t\t\t\t<\/span>\n\t\t\t\t\t<\/a>\n\t\t\t\t<\/div>\n\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<\/div>","protected":false},"excerpt":{"rendered":"<p>INDUSTRIAL COATING SCRATCH AND WEAR EVALUATION USING A TRIBOMETER Prepared by DUANJIE LI, PhD &amp; ANDREA HERRMANN INTRODUCTION Acrylic urethane paint is a type of fast-dry protective coating widely used in a variety of industrial applications, such as floor paint, auto paint, and others. When used as floor paint, it can serve areas with heavy [&hellip;]<\/p>\n","protected":false},"author":1,"featured_media":21169,"comment_status":"open","ping_status":"open","sticky":false,"template":"","format":"standard","meta":{"_exactmetrics_skip_tracking":false,"_exactmetrics_sitenote_active":false,"_exactmetrics_sitenote_note":"","_exactmetrics_sitenote_category":0,"footnotes":""},"categories":[7,348,349,337,351,335,373,345,346,336],"tags":[],"class_list":["post-20021","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-application-notes","category-friction-testing-coefficient-of-friction","category-laboratory-testing","category-mechanical-testing","category-profilometry-roughness-finish","category-profilometry-testing","category-rotational-tribology","category-scratch-testing-adhesive-failure","category-scratch-testing-cohesive-failure","category-tribology-testing"],"_links":{"self":[{"href":"https:\/\/nanovea.com\/ko\/wp-json\/wp\/v2\/posts\/20021","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/nanovea.com\/ko\/wp-json\/wp\/v2\/posts"}],"about":[{"href":"https:\/\/nanovea.com\/ko\/wp-json\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"https:\/\/nanovea.com\/ko\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/nanovea.com\/ko\/wp-json\/wp\/v2\/comments?post=20021"}],"version-history":[{"count":42,"href":"https:\/\/nanovea.com\/ko\/wp-json\/wp\/v2\/posts\/20021\/revisions"}],"predecessor-version":[{"id":23862,"href":"https:\/\/nanovea.com\/ko\/wp-json\/wp\/v2\/posts\/20021\/revisions\/23862"}],"wp:featuredmedia":[{"embeddable":true,"href":"https:\/\/nanovea.com\/ko\/wp-json\/wp\/v2\/media\/21169"}],"wp:attachment":[{"href":"https:\/\/nanovea.com\/ko\/wp-json\/wp\/v2\/media?parent=20021"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"https:\/\/nanovea.com\/ko\/wp-json\/wp\/v2\/categories?post=20021"},{"taxonomy":"post_tag","embeddable":true,"href":"https:\/\/nanovea.com\/ko\/wp-json\/wp\/v2\/tags?post=20021"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}