{"id":8344,"date":"2020-05-11T05:07:45","date_gmt":"2020-05-11T05:07:45","guid":{"rendered":"https:\/\/nanovea.com\/?p=8344"},"modified":"2023-11-13T22:17:52","modified_gmt":"2023-11-13T22:17:52","slug":"%e3%83%96%e3%83%ad%e3%83%83%e3%82%af%e3%83%bb%e3%82%aa%e3%83%b3%e3%83%bb%e3%83%aa%e3%83%b3%e3%82%b0%e3%83%bb%e3%82%b9%e3%83%a9%e3%82%a4%e3%83%89%e3%83%bb%e3%82%a6%e3%82%a7%e3%82%a2%e8%a9%95%e4%be%a1","status":"publish","type":"post","link":"https:\/\/nanovea.com\/ja\/block-on-ring-sliding-wear-evaluation\/","title":{"rendered":"\u30d6\u30ed\u30c3\u30af\u30fb\u30aa\u30f3\u30fb\u30ea\u30f3\u30b0\u6469\u8017\u8a66\u9a13"},"content":{"rendered":"<div data-elementor-type=\"wp-post\" data-elementor-id=\"8344\" class=\"elementor elementor-8344\" data-elementor-post-type=\"post\">\n\t\t\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-3a9803e6 elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"3a9803e6\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-13caf891\" data-id=\"13caf891\" data-element_type=\"column\" data-settings=\"{&quot;background_background&quot;:&quot;classic&quot;}\">\n\t\t\t<div class=\"elementor-widget-wrap\">\n\t\t\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-1a5e82a6 elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"1a5e82a6\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-77960ac2\" data-id=\"77960ac2\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-634241d9 elementor-widget elementor-widget-text-editor\" data-id=\"634241d9\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p style=\"text-align: left; color: #1b96cf; font-size: 24px; line-height: 30px;\"><strong><em>\u30d6\u30ed\u30c3\u30af\u30fb\u30aa\u30f3\u30fb\u30ea\u30f3\u30b0\u306e\u6469\u8017\u8a55\u4fa1\u306e\u91cd\u8981\u6027<\/em><u><i><br \/><\/i><\/u><\/strong><\/p><div>\u647a\u52d5\u6469\u8017\u3068\u306f\u3001\u8377\u91cd\u304c\u304b\u304b\u3063\u305f\u72b6\u614b\u3067\u30012\u3064\u306e\u6750\u6599\u304c\u63a5\u89e6\u90e8\u3067\u4e92\u3044\u306b\u6ed1\u308a\u3001\u6750\u6599\u304c\u5f90\u3005\u306b\u5931\u308f\u308c\u308b\u3053\u3068\u3067\u3042\u308b\u3002\u81ea\u52d5\u8eca\u3001\u822a\u7a7a\u5b87\u5b99\u3001\u77f3\u6cb9\u30fb\u30ac\u30b9\u306a\u3069\u3001\u6a5f\u68b0\u3084\u30a8\u30f3\u30b8\u30f3\u304c\u7a3c\u50cd\u3057\u3066\u3044\u308b\u69d8\u3005\u306a\u7523\u696d\u3067\u5fc5\u7136\u7684\u306b\u767a\u751f\u3059\u308b\u3002\u3053\u306e\u3088\u3046\u306a\u647a\u52d5\u904b\u52d5\u306f\u3001\u8868\u9762\u3067\u306e\u6df1\u523b\u306a\u6a5f\u68b0\u7684\u6469\u8017\u3084\u6750\u6599\u79fb\u52d5\u3092\u5f15\u304d\u8d77\u3053\u3057\u3001\u751f\u7523\u52b9\u7387\u3084\u6a5f\u68b0\u6027\u80fd\u306e\u4f4e\u4e0b\u3001\u3042\u308b\u3044\u306f\u6a5f\u68b0\u306e\u7834\u640d\u306b\u3064\u306a\u304c\u308b\u53ef\u80fd\u6027\u304c\u3042\u308b\u3002<\/div><div>\u00a0<\/div><p>\u00a0<\/p><div>\u6ed1\u308a\u6469\u8017\u306b\u306f\u3001\u51dd\u7740\u6469\u8017\u3001\u4e8c\u4f53\u6469\u8017\u3001\u4e09\u4f53\u6469\u8017\u3001\u75b2\u52b4\u6469\u8017\u306a\u3069\u3001\u63a5\u89e6\u9762\u3067\u767a\u751f\u3059\u308b\u8907\u96d1\u306a\u6469\u8017\u30e1\u30ab\u30cb\u30ba\u30e0\u304c\u95a2\u4e0e\u3059\u308b\u3053\u3068\u304c\u3088\u304f\u3042\u308a\u307e\u3059\u3002\u6750\u6599\u306e\u6469\u8017\u6319\u52d5\u306f\u3001\u901a\u5e38\u306e\u8377\u91cd\u3001\u901f\u5ea6\u3001\u8150\u98df\u3001\u6f64\u6ed1\u306a\u3069\u306e\u4f5c\u696d\u74b0\u5883\u306b\u5927\u304d\u304f\u5f71\u97ff\u3055\u308c\u307e\u3059\u3002\u591a\u7528\u9014\u306a <a href=\"https:\/\/nanovea.com\/tribometers\/\">\u30c8\u30e9\u30a4\u30dc\u30e1\u30fc\u30bf <\/a>\u3055\u307e\u3056\u307e\u306a\u73fe\u5b9f\u7684\u306a\u4f5c\u696d\u6761\u4ef6\u3092\u30b7\u30df\u30e5\u30ec\u30fc\u30c8\u3067\u304d\u308b\u305f\u3081\u3001\u6469\u8017\u8a55\u4fa1\u306b\u6700\u9069\u3067\u3059\u3002<br \/>\u30d6\u30ed\u30c3\u30af \u30aa\u30f3 \u30ea\u30f3\u30b0 (ASTM G77) \u8a66\u9a13\u306f\u3001\u3055\u307e\u3056\u307e\u306a\u30b7\u30df\u30e5\u30ec\u30fc\u30b7\u30e7\u30f3\u6761\u4ef6\u3067\u6750\u6599\u306e\u6ed1\u308a\u6469\u8017\u6319\u52d5\u3092\u8a55\u4fa1\u3059\u308b\u5e83\u304f\u4f7f\u7528\u3055\u308c\u3066\u3044\u308b\u624b\u6cd5\u3067\u3001\u7279\u5b9a\u306e\u30c8\u30e9\u30a4\u30dc\u30ed\u30b8\u30fc\u7528\u9014\u306b\u304a\u3051\u308b\u6750\u6599\u30ab\u30c3\u30d7\u30eb\u306e\u4fe1\u983c\u3067\u304d\u308b\u30e9\u30f3\u30af\u4ed8\u3051\u3092\u53ef\u80fd\u306b\u3057\u307e\u3059\u3002<\/div><div>\u00a0<\/div><div>\u00a0<\/div><p>\u00a0<\/p><p style=\"text-align: left; color: #1b96cf; font-size: 24px; line-height: 30px;\"><strong><em>\u6e2c\u5b9a\u76ee\u7684<\/em><u><i><br \/><\/i><\/u><\/strong><\/p><p>\u3053\u306e\u30a2\u30d7\u30ea\u30b1\u30fc\u30b7\u30e7\u30f3\u3067\u306f\u3001\u30ca\u30ce\u30d9\u30a2\u30e1\u30ab\u30cb\u30ab\u30eb\u30c6\u30b9\u30bf\u30fc\u304c\u3001\u30b9\u30c6\u30f3\u30ec\u30b9\u92fcSS304\u3068\u30a2\u30eb\u30df\u30cb\u30a6\u30e0Al6061\u91d1\u5c5e\u5408\u91d1\u30b5\u30f3\u30d7\u30eb\u306eYS\u3068UTS\u3092\u6e2c\u5b9a\u3057\u3066\u3044\u307e\u3059\u3002\u3053\u308c\u3089\u306e\u30b5\u30f3\u30d7\u30eb\u306f\u3001\u30ca\u30ce\u30d9\u30a2\u306e\u5727\u75d5\u6cd5\u306e\u4fe1\u983c\u6027\u3092\u793a\u3059\u3001\u4e00\u822c\u7684\u306b\u8a8d\u8b58\u3055\u308c\u3066\u3044\u308bYS\u3068UTS\u306e\u5024\u3067\u9078\u3070\u308c\u307e\u3057\u305f\u3002<\/p><p>\u00a0<\/p><div style=\"text-align: center;\"><a href=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/05\/Figure-1.png\"><img fetchpriority=\"high\" decoding=\"async\" class=\"alignnone size-full wp-image-8348\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/05\/Figure-1.png\" alt=\"\" width=\"648\" height=\"408\" \/><\/a><\/div><p>S-10 \u30ea\u30f3\u30b0\u4e0a\u306e H-30 \u30d6\u30ed\u30c3\u30af\u306e\u6ed1\u308a\u6469\u8017\u6319\u52d5\u306f\u3001Block-on-Ring \u30e2\u30b8\u30e5\u30fc\u30eb\u3092\u4f7f\u7528\u3059\u308b Nanovea \u306e\u30c8\u30e9\u30a4\u30dc\u30e1\u30fc\u30bf\u306b\u3088\u3063\u3066\u8a55\u4fa1\u3055\u308c\u307e\u3057\u305f\u3002 H-30 \u30d6\u30ed\u30c3\u30af\u306f\u786c\u5ea6 30HRC \u306e 01 \u5de5\u5177\u92fc\u3067\u4f5c\u3089\u308c\u3066\u3044\u307e\u3059\u304c\u3001S-10 \u30ea\u30f3\u30b0\u306f\u8868\u9762\u786c\u5ea6 58 \uff5e 63 HRC \u306e\u92fc\u30bf\u30a4\u30d7 4620\u3001\u30ea\u30f3\u30b0\u76f4\u5f84\u7d04 34.98 mm \u3067\u3059\u3002\u6469\u8017\u6319\u52d5\u3078\u306e\u5f71\u97ff\u3092\u8abf\u67fb\u3059\u308b\u305f\u3081\u306b\u3001\u4e7e\u71e5\u3057\u305f\u6f64\u6ed1\u74b0\u5883\u3067\u30d6\u30ed\u30c3\u30af \u30aa\u30f3 \u30ea\u30f3\u30b0 \u30c6\u30b9\u30c8\u304c\u5b9f\u884c\u3055\u308c\u307e\u3057\u305f\u3002\u6f64\u6ed1\u8a66\u9a13\u306f USP \u91cd\u9271\u6cb9\u3067\u5b9f\u65bd\u3055\u308c\u307e\u3057\u305f\u3002 Nanovea \u306e\u6469\u8017\u75d5\u8de1\u3092\u8abf\u67fb\u3057\u307e\u3057\u305f\u3002 <a href=\"https:\/\/nanovea.com\/profilometers\/\">3D\u975e\u63a5\u89e6\u8868\u9762\u5f62\u72b6\u8a08<\/a>\u3002\u8a66\u9a13\u30d1\u30e9\u30e1\u30fc\u30bf\u3092\u8868 1 \u306b\u307e\u3068\u3081\u307e\u3059\u3002\u6469\u8017\u7387 (K) \u306f\u3001\u5f0f K=V\/(F\u00d7s) \u3092\u4f7f\u7528\u3057\u3066\u8a55\u4fa1\u3057\u307e\u3057\u305f\u3002\u3053\u3053\u3067\u3001V \u306f\u6469\u8017\u91cf\u3001F \u306f\u5782\u76f4\u8377\u91cd\u3001s \u306f\u6ed1\u308a\u8ddd\u96e2\u3067\u3059\u3002<\/p><p>\u00a0<\/p><div style=\"text-align: center;\"><a href=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/05\/Table-1.png\"><img decoding=\"async\" class=\"alignnone size-full wp-image-8349\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/05\/Table-1.png\" alt=\"\" width=\"450\" height=\"106\" \/><\/a><\/div><p>\u00a0<\/p><p style=\"text-align: left; color: #1b96cf; font-size: 24px; line-height: 30px;\"><strong><em>\u7d50\u679c\u304a\u3088\u3073\u8003\u5bdf<\/em><u><i><br \/><\/i><\/u><\/strong><\/p><p style=\"margin: 0in; margin-bottom: .0001pt;\"><span style=\"font-family: 'Arial',sans-serif;\">\u56f3 2 \u306f\u3001\u4e7e\u71e5\u74b0\u5883\u3068\u6f64\u6ed1\u74b0\u5883\u3067\u306e\u30d6\u30ed\u30c3\u30af\u30aa\u30f3\u30ea\u30f3\u30b0 \u30c6\u30b9\u30c8\u306e\u6469\u64e6\u4fc2\u6570 (COF) \u3092\u6bd4\u8f03\u3057\u3066\u3044\u307e\u3059\u3002\u4e7e\u71e5\u3057\u305f\u74b0\u5883\u3067\u306f\u3001\u6f64\u6ed1\u3055\u308c\u305f\u74b0\u5883\u3088\u308a\u3082\u30d6\u30ed\u30c3\u30af\u306e\u6469\u64e6\u304c\u5927\u5e45\u306b\u5927\u304d\u304f\u306a\u308a\u307e\u3059\u3002 COF<br \/>\u6700\u521d\u306e 50 \u56de\u8ee2\u306e\u306a\u3089\u3057\u671f\u9593\u4e2d\u306b\u5909\u52d5\u3057\u3001\u6b8b\u308a\u306e 200 \u56de\u8ee2\u6469\u8017\u30c6\u30b9\u30c8\u3067\u306f\u7d04 0.8 \u306e\u4e00\u5b9a COF \u306b\u9054\u3057\u307e\u3059\u3002\u6bd4\u8f03\u3059\u308b\u3068\u3001USP \u91cd\u9271\u6cb9\u6f64\u6ed1\u3067\u5b9f\u884c\u3055\u308c\u305f\u30d6\u30ed\u30c3\u30af \u30aa\u30f3 \u30ea\u30f3\u30b0 \u30c6\u30b9\u30c8\u306f\u3001500,000 \u56de\u8ee2\u6469\u8017\u30c6\u30b9\u30c8\u5168\u4f53\u3092\u901a\u3058\u3066 0.09 \u3068\u3044\u3046\u4f4e\u3044 COF \u3092\u4e00\u5b9a\u306b\u793a\u3057\u307e\u3057\u305f\u3002\u6f64\u6ed1\u5264\u306f\u3001\u8868\u9762\u9593\u306e COF \u3092\u6700\u5927 90 \u5206\u306e 1 \u306b\u5927\u5e45\u306b\u524a\u6e1b\u3057\u307e\u3059\u3002<\/span><\/p><p style=\"margin: 0in; margin-bottom: .0001pt;\">\u00a0<\/p><p>\u56f33\uff0c\u56f34\u306b\u4e7e\u5f0f\u304a\u3088\u3073\u6f64\u6ed1\u5f0f\u6469\u8017\u8a66\u9a13\u5f8c\u306e\u30d6\u30ed\u30c3\u30af\u306e\u6469\u8017\u75d5\u306e\u5149\u5b66\u753b\u50cf\u3068\u65ad\u97622\u6b21\u5143\u30d7\u30ed\u30d5\u30a3\u30fc\u30eb\u3092\u793a\u3059\u3002\u307e\u305f\uff0c\u6469\u8017\u75d5\u306e\u4f53\u7a4d\u3068\u6469\u8017\u901f\u5ea6\u3092\u88682\u306b\u793a\u3059\u300272rpm\u306e\u4f4e\u56de\u8ee2\u6570\u3067200\u56de\u8ee2\u3055\u305b\u305f\u4e7e\u5f0f\u6469\u8017\u8a66\u9a13\u5f8c\u306e\u30b9\u30c1\u30fc\u30eb\u30d6\u30ed\u30c3\u30af\u306f\u30019.45mm\u02d9\u3068\u5927\u304d\u306a\u6469\u8017\u75d5\u4f53\u7a4d\u3092\u793a\u3057\u3066\u3044\u307e\u3059\u3002\u3053\u308c\u306b\u5bfe\u3057\u3001\u9271\u7269\u6cb9\u6f64\u6ed1\u5264\u3092\u7528\u3044\u3066197rpm\u306e\u9ad8\u901f\u56de\u8ee2\u306750\u4e07\u56de\u8ee2\u3055\u305b\u305f\u6469\u8017\u8a66\u9a13\u3067\u306f\u30010.03mm\u02d9\u3068\u5927\u5e45\u306b\u5c0f\u3055\u3044\u6469\u8017\u75d5\u304c\u5f62\u6210\u3055\u308c\u307e\u3057\u305f\u3002<\/p><p>\u00a0<\/p><p style=\"margin: 0in; margin-bottom: .0001pt;\"><span style=\"font-family: 'Arial',sans-serif;\"><br \/>\u56f33\u306f\u3001\u6f64\u6ed1\u6469\u8017\u8a66\u9a13\u3067\u306e\u7a4f\u3084\u304b\u306a\u6469\u8017\u306b\u6bd4\u3079\u3001\u4e7e\u5f0f\u6469\u8017\u8a66\u9a13\u3067\u306e\u6fc0\u3057\u3044\u6469\u8017\u306e\u69d8\u5b50\u3092\u793a\u3057\u3066\u3044\u307e\u3059\u3002\u4e7e\u5f0f\u6469\u8017\u8a66\u9a13\u3067\u767a\u751f\u3059\u308b\u9ad8\u71b1\u3068\u6fc0\u3057\u3044\u632f\u52d5\u306f\u3001\u91d1\u5c5e\u7247\u306e\u9178\u5316\u3092\u4fc3\u9032\u3057\u3001\u6fc0\u3057\u30443\u4f53\u6469\u8017\u3092\u5f15\u304d\u8d77\u3053\u3057\u307e\u3059\u3002\u6f64\u6ed1\u6469\u8017\u8a66\u9a13\u3067\u306f\u3001\u9271\u6cb9\u304c\u6469\u64e6\u3092\u6e1b\u3089\u3057\u3001\u63a5\u89e6\u9762\u3092\u51b7\u5374\u3057\u3001\u6469\u8017\u4e2d\u306b\u751f\u3058\u305f\u6469\u8017\u7c89\u3092\u904b\u3073\u53bb\u308a\u307e\u3059\u3002\u3053\u306e\u7d50\u679c\u3001\u6469\u8017\u91cf\u306f\u7d048\u00d710\u02c6\u3068\u5927\u5e45\u306b\u6e1b\u5c11\u3057\u305f\u3002\u3053\u306e\u3088\u3046\u306a\u74b0\u5883\u306b\u3088\u308b\u8010\u6469\u8017\u6027\u306e\u5927\u304d\u306a\u9055\u3044\u306f\u3001\u73fe\u5b9f\u7684\u306a\u4f7f\u7528\u6761\u4ef6\u4e0b\u3067\u306e\u9069\u5207\u306a\u6ed1\u308a\u6469\u8017\u30b7\u30df\u30e5\u30ec\u30fc\u30b7\u30e7\u30f3\u306e\u91cd\u8981\u6027\u3092\u793a\u3057\u3066\u3044\u308b\u3002<\/span><\/p><p>\u00a0<\/p><p style=\"margin: 0in; margin-bottom: .0001pt;\"><span style=\"font-family: 'Arial',sans-serif;\"><br \/>\u8a66\u9a13\u6761\u4ef6\u306b\u308f\u305a\u304b\u306a\u5909\u5316\u304c\u52a0\u308f\u308b\u3068\u3001\u6469\u8017\u306e\u6319\u52d5\u304c\u5927\u304d\u304f\u5909\u5316\u3059\u308b\u3053\u3068\u304c\u3042\u308a\u307e\u3059\u3002\u30ca\u30ce\u30d9\u30a2\u306e\u30c8\u30e9\u30a4\u30dc\u30e1\u30fc\u30bf\u306f\u6c4e\u7528\u6027\u304c\u9ad8\u3044\u305f\u3081\u3001\u9ad8\u6e29\u3001\u6f64\u6ed1\u3001\u30c8\u30e9\u30a4\u30dc\u30b3\u30ed\u30fc\u30b8\u30e7\u30f3\u306e\u5404\u6761\u4ef6\u3067\u6469\u8017\u6e2c\u5b9a\u304c\u53ef\u80fd\u3067\u3059\u3002\u9ad8\u5ea6\u306a\u30e2\u30fc\u30bf\u30fc\u306b\u3088\u308b\u6b63\u78ba\u306a\u901f\u5ea6\u304a\u3088\u3073\u4f4d\u7f6e\u5236\u5fa1\u306b\u3088\u308a\u30010.001\uff5e5000rpm\u306e\u901f\u5ea6\u3067\u6469\u8017\u8a66\u9a13\u3092\u884c\u3046\u3053\u3068\u304c\u3067\u304d\u308b\u305f\u3081\u3001\u7814\u7a76\/\u8a66\u9a13\u30e9\u30dc\u306b\u3068\u3063\u3066\u3001\u3055\u307e\u3056\u307e\u306a\u2fb0\u547d\u6761\u4ef6\u3067\u306e\u6469\u8017\u3092\u8abf\u3079\u308b\u305f\u3081\u306e\u7406\u60f3\u7684\u306a\u30c4\u30fc\u30eb\u3068\u306a\u3063\u3066\u3044\u307e\u3059\u3002<\/span><\/p><p style=\"margin: 0in; margin-bottom: .0001pt;\">\u00a0<\/p><p>\u8a66\u6599\u306e\u8868\u9762\u72b6\u614b\u306f\u3001Nanovea\u793e\u306e\u975e\u63a5\u89e6\u578b\u5149\u5b66\u5f0f\u30d7\u30ed\u30a4\u30aa\u30e1\u30fc\u30bf\u30fc\u3067\u691c\u67fb\u3057\u305f\u3002\u56f35\u306f\u3001\u6469\u8017\u8a66\u9a13\u5f8c\u306e\u30ea\u30f3\u30b0\u306e\u8868\u9762\u5f62\u614b\u3092\u793a\u3057\u3066\u3044\u307e\u3059\u3002\u647a\u52d5\u6469\u8017\u306b\u3088\u308a\u751f\u3058\u305f\u8868\u9762\u5f62\u614b\u3068\u7c97\u3055\u3092\u3088\u308a\u826f\u304f\u8868\u73fe\u3059\u308b\u305f\u3081\u306b\u3001\u5186\u7b52\u5f62\u72b6\u3092\u9664\u53bb\u3057\u3066\u3044\u307e\u3059\u3002200\u56de\u8ee2\u306e\u4e7e\u5f0f\u6469\u8017\u8a66\u9a13\u3067\u306f\u30013\u4f53\u6469\u8017\u306b\u3088\u308a\u8457\u3057\u3044\u8868\u9762\u8352\u308c\u304c\u767a\u751f\u3057\u307e\u3057\u305f\u3002\u4e7e\u5f0f\u6469\u8017\u8a66\u9a13\u5f8c\u306e\u30d6\u30ed\u30c3\u30af\u3068\u30ea\u30f3\u30b0\u306e\u7c97\u3055Ra\u306f\u3001\u305d\u308c\u305e\u308c14.1\u03bcm\u306818.1\u03bcm\u3067\u3042\u308b\u306e\u306b\u5bfe\u3057\u3001\u3088\u308a\u9ad8\u901f\u306e50\u4e07\u56de\u8ee2\u6f64\u6ed1\u6469\u8017\u8a66\u9a13\u3067\u306f5.7\u03bcm\u30689.1\u03bcm\u3068\u306a\u308a\u307e\u3057\u305f\u3002\u3053\u306e\u30c6\u30b9\u30c8\u306f\u3001\u30d4\u30b9\u30c8\u30f3\u30ea\u30f3\u30b0\u3068\u30b7\u30ea\u30f3\u30c0\u30fc\u306e\u63a5\u89e6\u9762\u306b\u9069\u5207\u306a\u6f64\u6ed1\u3092\u884c\u3046\u3053\u3068\u306e\u91cd\u8981\u6027\u3092\u793a\u3057\u3066\u3044\u307e\u3059\u3002\u6fc0\u3057\u3044\u6469\u8017\u306f\u3001\u7121\u6f64\u6ed1\u3067\u306f\u63a5\u89e6\u9762\u3092\u7d20\u65e9\u304f\u640d\u50b7\u3055\u305b\u3001\u4e0d\u53ef\u9006\u7684\u306a\u30b5\u30fc\u30d3\u30b9\u54c1\u8cea\u306e\u52a3\u5316\u3001\u3055\u3089\u306b\u306f\u30a8\u30f3\u30b8\u30f3\u306e\u7834\u640d\u306b\u3064\u306a\u304c\u308b\u3002<\/p><p>\u00a0<\/p><p style=\"margin: 0in; margin-bottom: .0001pt;\"><span style=\"font-family: 'Arial',sans-serif; color: #1c1e29;\">\u00a0<\/span><\/p><div style=\"text-align: center;\"><p><a href=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/05\/Figure-2-and-3.png\"><img decoding=\"async\" class=\"alignnone size-full wp-image-8350\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/05\/Figure-2-and-3.png\" alt=\"\" width=\"574\" height=\"847\" \/><\/a><\/p><p><a href=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/05\/Figure-4-and-Table-2.png\"><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-8351\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/05\/Figure-4-and-Table-2.png\" alt=\"\" width=\"671\" height=\"860\" \/><\/a><\/p><\/div><p style=\"text-align: left; color: #1b96cf; font-size: 24px; line-height: 30px;\"><strong><em>\u307e\u3068\u3081<\/em><u><i><br \/><\/i><\/u><\/strong><\/p><div style=\"text-align: center;\"><a href=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/05\/Conclusion-Pic.png\"><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-8352\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/05\/Conclusion-Pic.png\" alt=\"\" width=\"699\" height=\"491\" \/><\/a><\/div><p>\u3053\u306e\u7814\u7a76\u3067\u306f\u3001ASTM G77 \u898f\u683c\u306b\u6e96\u62e0\u3057\u305f\u30d6\u30ed\u30c3\u30af \u30aa\u30f3 \u30ea\u30f3\u30b0 \u30e2\u30b8\u30e5\u30fc\u30eb\u3092\u4f7f\u7528\u3057\u3066\u3001Nanovea \u306e\u30c8\u30e9\u30a4\u30dc\u30e1\u30fc\u30bf\u30fc\u3092\u4f7f\u7528\u3057\u3066\u30b9\u30c1\u30fc\u30eb\u91d1\u5c5e\u30ab\u30c3\u30d7\u30eb\u306e\u6ed1\u308a\u6469\u8017\u6319\u52d5\u3092\u8a55\u4fa1\u3059\u308b\u65b9\u6cd5\u3092\u7d39\u4ecb\u3057\u307e\u3059\u3002\u6f64\u6ed1\u5264\u306f\u3001\u6750\u6599\u5bfe\u306e\u6469\u8017\u7279\u6027\u306b\u304a\u3044\u3066\u91cd\u8981\u306a\u5f79\u5272\u3092\u679c\u305f\u3057\u307e\u3059\u3002\u9271\u6cb9\u306f\u3001H-30 \u30d6\u30ed\u30c3\u30af\u306e\u6469\u8017\u7387\u3092\u7d04 8\u00d710 \u5206\u306e 1 \u306b\u6e1b\u5c11\u3055\u305b\u3001COF \u3092\u7d04 90 \u5206\u306e 1 \u306b\u6e1b\u5c11\u3055\u305b\u307e\u3059\u3002 Nanovea \u306e\u30c8\u30e9\u30a4\u30dc\u30e1\u30fc\u30bf\u30fc\u306f\u591a\u7528\u9014\u6027\u3092\u5099\u3048\u3066\u3044\u308b\u305f\u3081\u3001\u3055\u307e\u3056\u307e\u306a\u6f64\u6ed1\u3001\u9ad8\u6e29\u3001\u6469\u64e6\u8150\u98df\u6761\u4ef6\u4e0b\u3067\u306e\u6469\u8017\u6319\u52d5\u3092\u6e2c\u5b9a\u3059\u308b\u305f\u3081\u306e\u7406\u60f3\u7684\u306a\u30c4\u30fc\u30eb\u3068\u306a\u3063\u3066\u3044\u307e\u3059\u3002<\/p><p>Nanovea \u306e\u30c8\u30e9\u30a4\u30dc\u30e1\u30fc\u30bf\u30fc\u306f\u3001ISO \u304a\u3088\u3073 ASTM \u6e96\u62e0\u306e\u56de\u8ee2\u30e2\u30fc\u30c9\u304a\u3088\u3073\u76f4\u7dda\u30e2\u30fc\u30c9\u3092\u4f7f\u7528\u3057\u3066\u3001\u6b63\u78ba\u3067\u518d\u73fe\u6027\u306e\u3042\u308b\u6469\u8017\u304a\u3088\u3073\u6469\u64e6\u8a66\u9a13\u3092\u63d0\u4f9b\u3057\u307e\u3059\u3002\u307e\u305f\u3001\u30aa\u30d7\u30b7\u30e7\u30f3\u306e\u9ad8\u6e29\u6469\u8017\u3001\u6f64\u6ed1\u3001\u304a\u3088\u3073\u6469\u64e6\u8150\u98df\u30e2\u30b8\u30e5\u30fc\u30eb\u3082 1 \u3064\u306e\u4e8b\u524d\u7d71\u5408\u30b7\u30b9\u30c6\u30e0\u3067\u5229\u7528\u3067\u304d\u307e\u3059\u3002 Nanovea \u306e\u6bd4\u985e\u306e\u306a\u3044\u88fd\u54c1\u7fa4\u306f\u3001\u8584\u3044\u304b\u539a\u3044\u304b\u3001\u67d4\u3089\u304b\u3044\u304b\u786c\u3044\u30b3\u30fc\u30c6\u30a3\u30f3\u30b0\u3001\u30d5\u30a3\u30eb\u30e0\u3001\u304a\u3088\u3073\u57fa\u6750\u306e\u3042\u3089\u3086\u308b\u7bc4\u56f2\u306e\u30c8\u30e9\u30a4\u30dc\u30ed\u30b8\u30fc\u7279\u6027\u3092\u6c7a\u5b9a\u3059\u308b\u305f\u3081\u306e\u7406\u60f3\u7684\u306a\u30bd\u30ea\u30e5\u30fc\u30b7\u30e7\u30f3\u3067\u3059\u3002<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-d39e8a2 elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"d39e8a2\" data-element_type=\"section\" data-settings=\"{&quot;background_background&quot;:&quot;classic&quot;}\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-a5d0b1d\" data-id=\"a5d0b1d\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-1b82dad elementor-widget elementor-widget-heading\" data-id=\"1b82dad\" data-element_type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\"><b>\u3055\u3066\u3001\u6b21\u306f\u30a2\u30d7\u30ea\u30b1\u30fc\u30b7\u30e7\u30f3\u306b\u3064\u3044\u3066\u3067\u3059\u3002<\/b><\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-414bcdf live-chat elementor-align-center elementor-widget elementor-widget-button\" data-id=\"414bcdf\" data-element_type=\"widget\" data-widget_type=\"button.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<div class=\"elementor-button-wrapper\">\n\t\t\t\t\t<a class=\"elementor-button elementor-button-link elementor-size-md\" href=\"https:\/\/nanovea.com\/contact\/live-chat\/\" id=\"live-chat\">\n\t\t\t\t\t\t<span class=\"elementor-button-content-wrapper\">\n\t\t\t\t\t\t\t\t\t<span class=\"elementor-button-text\">\u30e9\u30a4\u30d6\u30c1\u30e3\u30c3\u30c8<\/span>\n\t\t\t\t\t<\/span>\n\t\t\t\t\t<\/a>\n\t\t\t\t<\/div>\n\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<\/div>","protected":false},"excerpt":{"rendered":"<p>IMPORTANCE OF BLOCK-ON-RING WEAR EVALUATION Sliding wear is the progressive loss of material that results from two materials sliding against each other at the contact area under load. It occurs inevitably in a wide variety of industries where machines and engines are in operation, including automotive, aerospace, oil &amp; gas and many others. Such sliding motion causes serious mechanical wear and material transfer at the surface, which may lead to reduced production efficiency, machine performance or even damage to the machine.\u00a0 \u00a0 Sliding wear often involves complex wear mechanisms taking place at the contact surface, such as adhesion wear, two-body abrasion, three-body abrasion and fatigue wear. The wear behavior of [&hellip;]<\/p>\n","protected":false},"author":1,"featured_media":11684,"comment_status":"open","ping_status":"open","sticky":false,"template":"","format":"standard","meta":{"_exactmetrics_skip_tracking":false,"_exactmetrics_sitenote_active":false,"_exactmetrics_sitenote_note":"","_exactmetrics_sitenote_category":0,"footnotes":""},"categories":[7,374,349,351,353,355,335,336],"tags":[],"class_list":["post-8344","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-application-notes","category-block-on-ring-tribology","category-laboratory-testing","category-profilometry-roughness-finish","category-profilometry-texture-grain","category-profilometry-volume-area","category-profilometry-testing","category-tribology-testing"],"_links":{"self":[{"href":"https:\/\/nanovea.com\/ja\/wp-json\/wp\/v2\/posts\/8344","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/nanovea.com\/ja\/wp-json\/wp\/v2\/posts"}],"about":[{"href":"https:\/\/nanovea.com\/ja\/wp-json\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"https:\/\/nanovea.com\/ja\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/nanovea.com\/ja\/wp-json\/wp\/v2\/comments?post=8344"}],"version-history":[{"count":19,"href":"https:\/\/nanovea.com\/ja\/wp-json\/wp\/v2\/posts\/8344\/revisions"}],"predecessor-version":[{"id":23411,"href":"https:\/\/nanovea.com\/ja\/wp-json\/wp\/v2\/posts\/8344\/revisions\/23411"}],"wp:featuredmedia":[{"embeddable":true,"href":"https:\/\/nanovea.com\/ja\/wp-json\/wp\/v2\/media\/11684"}],"wp:attachment":[{"href":"https:\/\/nanovea.com\/ja\/wp-json\/wp\/v2\/media?parent=8344"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"https:\/\/nanovea.com\/ja\/wp-json\/wp\/v2\/categories?post=8344"},{"taxonomy":"post_tag","embeddable":true,"href":"https:\/\/nanovea.com\/ja\/wp-json\/wp\/v2\/tags?post=8344"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}