{"id":7819,"date":"2020-02-11T14:38:38","date_gmt":"2020-02-11T14:38:38","guid":{"rendered":"https:\/\/nanovea.com\/?p=7819"},"modified":"2025-05-22T20:57:21","modified_gmt":"2025-05-22T20:57:21","slug":"%e6%b9%bf%e5%ba%a6%e5%8a%b9%e6%9e%9c-dlc%e3%82%b3%e3%83%bc%e3%83%86%e3%82%a3%e3%83%b3%e3%82%b0-%e3%83%88%e3%83%a9%e3%82%a4%e3%83%9c%e3%83%ad%e3%82%b8%e3%83%bc","status":"publish","type":"post","link":"https:\/\/nanovea.com\/ja\/humidity-effect-on-dlc-coating-tribology\/","title":{"rendered":"DLC\u819c\u306e\u30c8\u30e9\u30a4\u30dc\u30ed\u30b8\u30fc\u306b\u304a\u3051\u308b\u6e7f\u5ea6\u52b9\u679c"},"content":{"rendered":"<div data-elementor-type=\"wp-post\" data-elementor-id=\"7819\" class=\"elementor elementor-7819\" data-elementor-post-type=\"post\">\n\t\t\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-3383a1d2 elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"3383a1d2\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-27e95971\" data-id=\"27e95971\" data-element_type=\"column\" data-settings=\"{&quot;background_background&quot;:&quot;classic&quot;}\">\n\t\t\t<div class=\"elementor-widget-wrap\">\n\t\t\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-26f0f9af elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"26f0f9af\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-ea7f871\" data-id=\"ea7f871\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-6c8704d7 elementor-widget elementor-widget-text-editor\" data-id=\"6c8704d7\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p style=\"text-align: left; color: #1b96cf; font-size: 24px;\">DLC\u306e\u6e7f\u5ea6\u4e0b\u3067\u306e\u6469\u8017\u8a55\u4fa1\u306e\u91cd\u8981\u6027<strong><u><i><br>\n<\/i><\/u><\/strong><\/p>\n<p>\u30c0\u30a4\u30e4\u30e2\u30f3\u30c9 \u30e9\u30a4\u30af \u30ab\u30fc\u30dc\u30f3 (DLC) \u30b3\u30fc\u30c6\u30a3\u30f3\u30b0\u306f\u3001\u5f37\u5316\u3055\u308c\u305f\u6469\u64e6\u7279\u6027\u3001\u3064\u307e\u308a\u512a\u308c\u305f\u8010\u6469\u8017\u6027\u3068\u975e\u5e38\u306b\u4f4e\u3044\u6469\u64e6\u4fc2\u6570 (COF) \u3092\u5099\u3048\u3066\u3044\u307e\u3059\u3002 DLC \u30b3\u30fc\u30c6\u30a3\u30f3\u30b0\u306f\u3001\u3055\u307e\u3056\u307e\u306a\u6750\u6599\u4e0a\u306b\u84b8\u7740\u3055\u308c\u308b\u3068\u30c0\u30a4\u30e4\u30e2\u30f3\u30c9\u306e\u7279\u6027\u3092\u4e0e\u3048\u307e\u3059\u3002\u6709\u5229\u306a\u6469\u64e6\u6a5f\u68b0\u7279\u6027\u306b\u3088\u308a\u3001DLC \u30b3\u30fc\u30c6\u30a3\u30f3\u30b0\u306f\u822a\u7a7a\u5b87\u5b99\u90e8\u54c1\u3001\u304b\u307f\u305d\u308a\u306e\u5203\u3001\u91d1\u5c5e\u5207\u524a\u5de5\u5177\u3001\u30d9\u30a2\u30ea\u30f3\u30b0\u3001\u30aa\u30fc\u30c8\u30d0\u30a4\u306e\u30a8\u30f3\u30b8\u30f3\u3001\u533b\u7642\u7528\u30a4\u30f3\u30d7\u30e9\u30f3\u30c8\u306a\u3069\u306e\u3055\u307e\u3056\u307e\u306a\u7523\u696d\u7528\u9014\u306b\u9069\u3057\u3066\u3044\u307e\u3059\u3002<\/p>\n<p>DLC \u30b3\u30fc\u30c6\u30a3\u30f3\u30b0\u306f\u3001\u9ad8\u771f\u7a7a\u304a\u3088\u3073\u4e7e\u71e5\u6761\u4ef6\u4e0b\u3067\u92fc\u7403\u306b\u5bfe\u3057\u3066\u975e\u5e38\u306b\u4f4e\u3044 COF (0.1 \u672a\u6e80) \u3092\u793a\u3057\u307e\u3059\u3002<sup>12<\/sup>.\u3057\u304b\u3057\u3001DLC\u30b3\u30fc\u30c6\u30a3\u30f3\u30b0\u306f\u74b0\u5883\u6761\u4ef6\u306e\u5909\u5316\u3001\u7279\u306b\u76f8\u5bfe\u6e7f\u5ea6\uff08RH\uff09\u306b\u654f\u611f\u3067\u3042\u308b\u3002<sup>3<\/sup>.\u6e7f\u5ea6\u3084\u9178\u7d20\u6fc3\u5ea6\u304c\u9ad8\u3044\u74b0\u5883\u3067\u306f\u3001COF\u304c\u5927\u5e45\u306b\u5897\u52a0\u3059\u308b\u53ef\u80fd\u6027\u304c\u3042\u308a\u307e\u3059\u3002<sup>4<\/sup>\u3002\u5236\u5fa1\u3055\u308c\u305f\u6e7f\u5ea6\u3067\u306e\u4fe1\u983c\u6027\u306e\u9ad8\u3044\u6469\u8017\u8a55\u4fa1\u306b\u3088\u308a\u3001\u30c8\u30e9\u30a4\u30dc\u30ed\u30b8\u30fc\u7528\u9014\u306b\u304a\u3051\u308b DLC \u30b3\u30fc\u30c6\u30a3\u30f3\u30b0\u306e\u73fe\u5b9f\u7684\u306a\u74b0\u5883\u6761\u4ef6\u304c\u30b7\u30df\u30e5\u30ec\u30fc\u30c8\u3055\u308c\u307e\u3059\u3002\u30e6\u30fc\u30b6\u30fc\u306f\u9069\u5207\u306a\u6bd4\u8f03\u3092\u884c\u3044\u3001\u5bfe\u8c61\u7528\u9014\u306b\u6700\u9069\u306aDLC\u30b3\u30fc\u30c6\u30a3\u30f3\u30b0\u3092\u9078\u629e\u3057\u307e\u3059\u3002<br>\n\u3055\u307e\u3056\u307e\u306a\u6e7f\u5ea6\u306b\u3055\u3089\u3055\u308c\u305fDLC\u306e\u6469\u8017\u6319\u52d5\u306e\u5909\u5316\u3002<br>\n<br><br><br><\/p>\n<p style=\"text-align: left; color: #1b96cf; font-size: 24px;\">\u6e2c\u5b9a\u76ee\u7684<\/p>\n<p>\u3053\u306e\u7814\u7a76\u3067\u306f Nanovea \u3092\u7d39\u4ecb\u3057\u307e\u3059 <a href=\"https:\/\/nanovea.com\/tribometers\/\">\u30c8\u30e9\u30a4\u30dc\u30e1\u30fc\u30bf <\/a>\u6e7f\u5ea6\u30b3\u30f3\u30c8\u30ed\u30fc\u30e9\u30fc\u3092\u5099\u3048\u305f\u3053\u306e\u30c4\u30fc\u30eb\u306f\u3001\u3055\u307e\u3056\u307e\u306a\u76f8\u5bfe\u6e7f\u5ea6\u306b\u304a\u3051\u308b DLC \u30b3\u30fc\u30c6\u30a3\u30f3\u30b0\u306e\u6469\u8017\u6319\u52d5\u3092\u8abf\u67fb\u3059\u308b\u306e\u306b\u6700\u9069\u306a\u30c4\u30fc\u30eb\u3067\u3059\u3002<\/p>\n<p style=\"margin: 0in; margin-bottom: .0001pt;\"><span style=\"font-family: 'Arial',sans-serif;\">&nbsp;<\/span><\/p>\n<div style=\"text-align: center;\"><a href=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/02\/meausrement-objective-picture.jpg\"><img fetchpriority=\"high\" decoding=\"async\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/02\/meausrement-objective-picture.jpg\" alt=\"\" width=\"978\" height=\"884\"><\/a><\/div>\n<p>&nbsp;<br>\n<br><br><br><\/p>\n<p style=\"text-align: left; color: #1b96cf; font-size: 24px;\">\u8a66\u9a13\u65b9\u6cd5<strong><u><i><br>\n<\/i><\/u><\/strong><\/p>\n<p>DLC \u30b3\u30fc\u30c6\u30a3\u30f3\u30b0\u306e\u8010\u6469\u64e6\u6027\u3068\u8010\u6469\u8017\u6027\u306f\u3001Nanovea Tribometer \u306b\u3088\u3063\u3066\u8a55\u4fa1\u3055\u308c\u307e\u3057\u305f\u3002\u30c6\u30b9\u30c8\u30d1\u30e9\u30e1\u30fc\u30bf\u3092\u8868 1 \u306b\u307e\u3068\u3081\u307e\u3059\u3002\u30c8\u30e9\u30a4\u30dc\u30c1\u30e3\u30f3\u30d0\u30fc\u306b\u53d6\u308a\u4ed8\u3051\u3089\u308c\u305f\u6e7f\u5ea6\u30b3\u30f3\u30c8\u30ed\u30fc\u30e9\u306f\u3001\u00b11% \u306e\u7cbe\u5ea6\u3067\u76f8\u5bfe\u6e7f\u5ea6 (RH) \u3092\u6b63\u78ba\u306b\u5236\u5fa1\u3057\u307e\u3057\u305f\u3002\u8a66\u9a13\u5f8c\u3001DLC \u30b3\u30fc\u30c6\u30a3\u30f3\u30b0\u306e\u6469\u8017\u75d5\u8de1\u3068 SiN \u30dc\u30fc\u30eb\u306e\u6469\u8017\u75d5\u3092\u5149\u5b66\u9855\u5fae\u93e1\u3092\u4f7f\u7528\u3057\u3066\u691c\u67fb\u3057\u307e\u3057\u305f\u3002<\/p>\n<p>\u6ce8: \u6f64\u6ed1\u5264\u3084\u9ad8\u6e29\u306a\u3069\u306e\u74b0\u5883\u6761\u4ef6\u4e0b\u3067\u3001\u3055\u307e\u3056\u307e\u306a\u6750\u6599\u306e\u30ab\u30c3\u30d7\u30ea\u30f3\u30b0\u306e\u6027\u80fd\u3092\u30b7\u30df\u30e5\u30ec\u30fc\u30c8\u3059\u308b\u305f\u3081\u306b\u3001\u4efb\u610f\u306e\u56fa\u4f53\u30dc\u30fc\u30eb\u6750\u6599\u3092\u9069\u7528\u3067\u304d\u307e\u3059\u3002<\/p>\n<p><br><br><a href=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/02\/Table-1-1.png\"><img decoding=\"async\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/02\/Table-1-1.png\" alt=\"\" width=\"821\" height=\"632\"><\/a><br>\n<br><br><br><\/p>\n<p style=\"text-align: left; color: #1b96cf; font-size: 24px;\">\u7d50\u679c\u304a\u3088\u3073\u8003\u5bdf<strong><u><i><br>\n<\/i><\/u><\/strong><\/p>\n<div><\/div>\n<p style=\"margin: 0in; margin-bottom: .0001pt;\"><span style=\"font-family: 'Arial',sans-serif;\">DLC\u30b3\u30fc\u30c6\u30a3\u30f3\u30b0\u306f\u3001\u4f4e\u6469\u64e6\u3067\u8010\u6469\u8017\u6027\u306b\u512a\u308c\u3066\u3044\u308b\u305f\u3081\u3001\u30c8\u30e9\u30a4\u30dc\u30ed\u30b8\u30fc\u7528\u9014\u306b\u6700\u9069\u3067\u3059\u3002DLC\u30b3\u30fc\u30c6\u30a3\u30f3\u30b0\u306e\u6469\u64e6\u306f\u3001\u56f32\u306b\u793a\u3059\u3088\u3046\u306a\u6e7f\u5ea6\u4f9d\u5b58\u6027\u306e\u6319\u52d5\u3092\u793a\u3057\u3066\u3044\u307e\u3059\u3002\u6bd4\u8f03\u7684\u4e7e\u71e5\u3057\u305f\u6761\u4ef6\u4e0b\uff0810% RH\uff09\u3067\u306f\u3001DLC\u30b3\u30fc\u30c6\u30a3\u30f3\u30b0\u306f\u6469\u8017\u8a66\u9a13\u4e2d\u3001\u7d040.05\u3068\u3044\u3046\u975e\u5e38\u306b\u4f4e\u3044COF\u3092\u793a\u3057\u307e\u3057\u305f\u3002RH\u304c30%\u307e\u3067\u4e0a\u6607\u3059\u308b\u3068\u3001DLC\u30b3\u30fc\u30c6\u30a3\u30f3\u30b0\u306f\u3001\u8a66\u9a13\u4e2d\u3001\u301c0.1\u306e\u4e00\u5b9a\u306eCOF\u3092\u793a\u3057\u307e\u3057\u305f\u3002COF\u306e\u521d\u671f\u6bb5\u968e\u306f\u3001RH\u304c50%\u4ee5\u4e0a\u306b\u4e0a\u6607\u3057\u305f\u6700\u521d\u306e2000\u56de\u8ee2\u3067\u89b3\u5bdf\u3055\u308c\u307e\u3059\u3002DLC\u30b3\u30fc\u30c6\u30a3\u30f3\u30b0\u306f\u3001RH\u304c50\u300170\u300190%\u306e\u3068\u304d\u306b\u305d\u308c\u305e\u308c\u301c0.20\u3001\u301c0.26\u3001\u301c0.33\u3068\u3044\u3046\u6700\u5927COF\u3092\u793a\u3059\u3002\u6163\u3089\u3057\u904b\u8ee2\u5f8c\u3001DLC\u30b3\u30fc\u30c6\u30a3\u30f3\u30b0\u306eCOF\u306f\u3001RH50\u300170\u300190%\u3067\u305d\u308c\u305e\u308c\u301c0.11\u30010.13\u30010.20\u3068\u4e00\u5b9a\u306b\u4fdd\u305f\u308c\u308b\u3002<\/span><\/p>\n<p style=\"margin: 0in; margin-bottom: .0001pt;\"><span style=\"font-family: 'Arial',sans-serif; color: #1c1e29;\">&nbsp;<\/span><\/p>\n<p><a href=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/02\/Figure-2.png\"><img decoding=\"async\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/02\/Figure-2.png\" alt=\"\" width=\"878\" height=\"719\"><\/a><\/p>\n<p><br><br>\u56f33\u306fSiN\u30dc\u30fc\u30eb\u306e\u6469\u8017\u75d5\u3001\u56f34\u306f\u6469\u8017\u8a66\u9a13\u5f8c\u306eDLC\u30b3\u30fc\u30c6\u30a3\u30f3\u30b0\u306e\u6469\u8017\u75d5\u3092\u6bd4\u8f03\u3057\u305f\u3082\u306e\u3067\u3042\u308b\u3002\u6e7f\u5ea6\u306e\u4f4e\u3044\u74b0\u5883\u306b\u3055\u3089\u3055\u308c\u305fDLC\u30b3\u30fc\u30c6\u30a3\u30f3\u30b0\u306e\u65b9\u304c\u3001\u6469\u8017\u75d5\u306e\u76f4\u5f84\u304c\u5c0f\u3055\u304f\u306a\u3063\u3066\u3044\u308b\u3053\u3068\u304c\u308f\u304b\u308b\u3002\u63a5\u89e6\u9762\u306b\u304a\u3044\u3066\u7e70\u308a\u8fd4\u3057\u647a\u52d5\u3059\u308b\u3053\u3068\u3067\uff0cSiN \u30dc\u30fc\u30eb\u8868\u9762\u306b\u8ee2\u5199 DLC \u5c64\u304c\u84c4\u7a4d\u3055\u308c\u308b\u3002\u3053\u306e\u6bb5\u968e\u3067\uff0cDLC \u88ab\u819c\u306f\u81ea\u8eab\u306e\u8ee2\u5199\u819c\u3068\u647a\u52d5\u3057\uff0c\u52b9\u7387\u7684\u306a\u6f64\u6ed1\u5264\u3068\u3057\u3066\u76f8\u5bfe\u904b\u52d5\u3092\u4fc3\u9032\u3057\uff0c\u305b\u3093\u65ad\u5909\u5f62\u306b\u3088\u308b\u3055\u3089\u306a\u308b\u8cea\u91cf\u6e1b\u5c11\u3092\u6291\u5236\u3057\u3066\u3044\u308b\u3053\u3068\u304c\u308f\u304b\u308b\u3002\u4f4eRH\u74b0\u5883\uff0810%\u308430%\u306a\u3069\uff09\u3067\u306f\uff0cSiN\u30dc\u30fc\u30eb\u306e\u6469\u8017\u75d5\u306b\u8ee2\u5199\u819c\u304c\u89b3\u5bdf\u3055\u308c\uff0c\u30dc\u30fc\u30eb\u306e\u6469\u8017\u904e\u7a0b\u304c\u6e1b\u901f\u3055\u308c\u308b\uff0e\u3053\u306e\u6469\u8017\u904e\u7a0b\u306f\u3001\u56f34\u306b\u793a\u3059\u3088\u3046\u306bDLC\u30b3\u30fc\u30c6\u30a3\u30f3\u30b0\u306e\u6469\u8017\u75d5\u306e\u5f62\u614b\u306b\u53cd\u6620\u3055\u308c\u308b\u3002\u3053\u308c\u306f\uff0c\u63a5\u89e6\u754c\u9762\u306b\u5b89\u5b9a\u3057\u305fDLC\u819c\u304c\u5f62\u6210\u3055\u308c\uff0c\u6469\u64e6\u3068\u6469\u8017\u901f\u5ea6\u304c\u5927\u5e45\u306b\u4f4e\u6e1b\u3055\u308c\u305f\u305f\u3081\u3067\u3042\u308b\u3002<br>\n<br><br><\/p>\n<div style=\"text-align: center;\"><a href=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/02\/Figure-3.png\"><img loading=\"lazy\" decoding=\"async\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/02\/Figure-3.png\" alt=\"\" width=\"551\" height=\"716\"><\/a><br>\n<br><br><a href=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/02\/Figure-4.png\">\n<\/a><p><a href=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/02\/Figure-4.png\"><img loading=\"lazy\" decoding=\"async\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/02\/Figure-4.png\" alt=\"\" width=\"556\" height=\"716\"><\/a><\/p><\/div>\n<p>&nbsp;<br>\n<br><br><\/p>\n<p style=\"text-align: left; color: #1b96cf; font-size: 24px;\">\u7d50\u8ad6<\/p>\n<p><br><a href=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/02\/Conclusion-photo.jpg\"><img loading=\"lazy\" decoding=\"async\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/02\/Conclusion-photo.jpg\" alt=\"\" width=\"1212\" height=\"656\"><\/a><\/p>\n<p><br><br>\u6e7f\u5ea6\u306f\u3001DLC \u30b3\u30fc\u30c6\u30a3\u30f3\u30b0\u306e\u6469\u64e6\u5b66\u7684\u6027\u80fd\u306b\u91cd\u8981\u306a\u5f79\u5272\u3092\u679c\u305f\u3057\u307e\u3059\u3002 DLC \u30b3\u30fc\u30c6\u30a3\u30f3\u30b0\u306f\u3001\u647a\u52d5\u76f8\u624b (\u3053\u306e\u7814\u7a76\u3067\u306f SiN \u30dc\u30fc\u30eb) \u306b\u8ee2\u5199\u3055\u308c\u305f\u5b89\u5b9a\u3057\u305f\u9ed2\u925b\u5c64\u306e\u5f62\u6210\u306b\u3088\u308a\u3001\u4e7e\u71e5\u72b6\u614b\u3067\u5927\u5e45\u306b\u5f37\u5316\u3055\u308c\u305f\u8010\u6469\u8017\u6027\u3068\u512a\u308c\u305f\u4f4e\u6469\u64e6\u3092\u5099\u3048\u3066\u3044\u307e\u3059\u3002 DLC \u30b3\u30fc\u30c6\u30a3\u30f3\u30b0\u306f\u3001\u305d\u308c\u81ea\u8eab\u306e\u8ee2\u5199\u5c64\u306b\u5bfe\u3057\u3066\u6ed1\u308a\u307e\u3059\u3002\u3053\u306e\u8ee2\u5199\u5c64\u306f\u52b9\u7387\u7684\u306a\u6f64\u6ed1\u5264\u3068\u3057\u3066\u6a5f\u80fd\u3057\u3001\u76f8\u5bfe\u904b\u52d5\u3092\u4fc3\u9032\u3057\u3001\u305b\u3093\u65ad\u5909\u5f62\u306b\u3088\u3063\u3066\u5f15\u304d\u8d77\u3053\u3055\u308c\u308b\u3055\u3089\u306a\u308b\u8cea\u91cf\u640d\u5931\u3092\u6291\u5236\u3057\u307e\u3059\u3002\u76f8\u5bfe\u6e7f\u5ea6\u304c\u4e0a\u6607\u3059\u308b\u3068\u3001SiN \u30dc\u30fc\u30eb\u4e0a\u306b\u819c\u304c\u89b3\u5bdf\u3055\u308c\u306a\u304f\u306a\u308a\u3001SiN \u30dc\u30fc\u30eb\u3068 DLC \u30b3\u30fc\u30c6\u30a3\u30f3\u30b0\u306e\u6469\u8017\u7387\u304c\u5897\u52a0\u3057\u307e\u3059\u3002<\/p>\n<p>Nanovea \u30c8\u30e9\u30a4\u30dc\u30e1\u30fc\u30bf\u30fc\u306f\u3001ISO \u304a\u3088\u3073 ASTM \u6e96\u62e0\u306e\u56de\u8ee2\u30e2\u30fc\u30c9\u304a\u3088\u3073\u76f4\u7dda\u30e2\u30fc\u30c9\u3092\u4f7f\u7528\u3057\u305f\u53cd\u5fa9\u53ef\u80fd\u306a\u6469\u8017\u304a\u3088\u3073\u6469\u64e6\u8a66\u9a13\u3092\u63d0\u4f9b\u3057\u30011 \u3064\u306e\u4e8b\u524d\u7d71\u5408\u30b7\u30b9\u30c6\u30e0\u3067\u5229\u7528\u53ef\u80fd\u306a\u30aa\u30d7\u30b7\u30e7\u30f3\u306e\u6e7f\u5ea6\u30e2\u30b8\u30e5\u30fc\u30eb\u3092\u5099\u3048\u3066\u3044\u307e\u3059\u3002\u3053\u308c\u306b\u3088\u308a\u3001\u30e6\u30fc\u30b6\u30fc\u306f\u3055\u307e\u3056\u307e\u306a\u6e7f\u5ea6\u3067\u306e\u4f5c\u696d\u74b0\u5883\u3092\u30b7\u30df\u30e5\u30ec\u30fc\u30c8\u3067\u304d\u3001\u3055\u307e\u3056\u307e\u306a\u4f5c\u696d\u6761\u4ef6\u4e0b\u3067\u306e\u6750\u6599\u306e\u30c8\u30e9\u30a4\u30dc\u30ed\u30b8\u30fc\u6319\u52d5\u3092\u5b9a\u91cf\u7684\u306b\u8a55\u4fa1\u3059\u308b\u305f\u3081\u306e\u7406\u60f3\u7684\u306a\u30c4\u30fc\u30eb\u3092\u30e6\u30fc\u30b6\u30fc\u306b\u63d0\u4f9b\u3067\u304d\u307e\u3059\u3002<\/p>\n<p><br><br>\u30ca\u30ce\u30d9\u30fc\u30b9\u30c8\u30e9\u30a4\u30dc\u30e1\u30fc\u30bf\u3068\u30e9\u30dc\u30b5\u30fc\u30d3\u30b9\u306b\u3064\u3044\u3066\u306e\u8a73\u7d30\u306f\u3053\u3061\u3089<br>\n<br>1 C. Donnet, Surf.Coat.Technol.100-101 (1998) 180.<br>\n<br>2 \u4e09\u597d\u548c\u5f66, B. Pohlchuck, K.W. Street, J.S. Zabinski, J.H. Sanders, A.A. Voevodin, R.L.C. Wu, Wear 225-229 (1999) 65.<br>\n<br>3 R. Gilmore, R. Hauert, Surf.Coat.Technol.133-134 (2000) 437.<br>\n<br>4 R. Memming, H.J. Tolle, P.E. Wierenga, Thin Solid Coatings 143 (1986) 31<br>\n<br><br><\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-c2b131b elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"c2b131b\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-a68c071\" data-id=\"a68c071\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-a25abb8 elementor-widget elementor-widget-heading\" data-id=\"a25abb8\" data-element_type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\">\u540c\u3058\u3088\u3046\u306a\u30a2\u30d7\u30ea\u30b1\u30fc\u30b7\u30e7\u30f3\u3092\u304a\u6301\u3061\u3067\u3059\u304b\uff1f<\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-70fdc0e elementor-align-justify open-chat elementor-widget elementor-widget-button\" data-id=\"70fdc0e\" data-element_type=\"widget\" data-widget_type=\"button.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<div class=\"elementor-button-wrapper\">\n\t\t\t\t\t<a class=\"elementor-button elementor-size-sm\" role=\"button\">\n\t\t\t\t\t\t<span class=\"elementor-button-content-wrapper\">\n\t\t\t\t\t\t\t\t\t<span class=\"elementor-button-text\">\u5c02\u9580\u5bb6\u306b\u76f8\u8ac7\u3059\u308b<\/span>\n\t\t\t\t\t<\/span>\n\t\t\t\t\t<\/a>\n\t\t\t\t<\/div>\n\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-3c53e1d elementor-align-justify button-quote elementor-widget elementor-widget-button\" data-id=\"3c53e1d\" data-element_type=\"widget\" data-widget_type=\"button.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<div class=\"elementor-button-wrapper\">\n\t\t\t\t\t<a class=\"elementor-button elementor-button-link elementor-size-sm\" href=\"https:\/\/nanovea.com\/contact-sales-form\/\" id=\"button-quote-bottom\">\n\t\t\t\t\t\t<span class=\"elementor-button-content-wrapper\">\n\t\t\t\t\t\t\t\t\t<span class=\"elementor-button-text\">\u4fa1\u683c\u3068\u8a73\u7d30\u3092\u7d20\u65e9\u304f\u5165\u624b<\/span>\n\t\t\t\t\t<\/span>\n\t\t\t\t\t<\/a>\n\t\t\t\t<\/div>\n\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<\/div>","protected":false},"excerpt":{"rendered":"<p>Importance of Wear Evaluation on DLC in Humidity Diamond-like carbon (DLC) coatings possess enhanced tribological properties, namely excellent wear resistance and a very low coefficient of friction (COF). DLC coatings impart diamond characteristics when deposited on different materials. Favorable tribo-mechanical properties make DLC coatings preferable in various industrial applications, such as aerospace parts, razor blades, metal cutting tools, bearings, motorcycle engines, and medical implants. DLC coatings exhibit very low COF (below 0.1) against steel balls under high vacuum and dry conditions\u001d\u001c12. However, DLC coatings are sensitive to environmental condition changes, particularly relative humidity (RH)3\u001b. Environments with high humidity and oxygen concentration may lead to significant increase in COF\u00194. Reliable wear [&hellip;]<\/p>\n","protected":false},"author":1,"featured_media":11695,"comment_status":"open","ping_status":"open","sticky":false,"template":"","format":"standard","meta":{"_exactmetrics_skip_tracking":false,"_exactmetrics_sitenote_active":false,"_exactmetrics_sitenote_note":"","_exactmetrics_sitenote_category":0,"footnotes":""},"categories":[7,382,349,372,373,336],"tags":[],"class_list":["post-7819","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-application-notes","category-humidity-gases-tribology","category-laboratory-testing","category-linear-tribology","category-rotational-tribology","category-tribology-testing"],"_links":{"self":[{"href":"https:\/\/nanovea.com\/ja\/wp-json\/wp\/v2\/posts\/7819","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/nanovea.com\/ja\/wp-json\/wp\/v2\/posts"}],"about":[{"href":"https:\/\/nanovea.com\/ja\/wp-json\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"https:\/\/nanovea.com\/ja\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/nanovea.com\/ja\/wp-json\/wp\/v2\/comments?post=7819"}],"version-history":[{"count":33,"href":"https:\/\/nanovea.com\/ja\/wp-json\/wp\/v2\/posts\/7819\/revisions"}],"predecessor-version":[{"id":24791,"href":"https:\/\/nanovea.com\/ja\/wp-json\/wp\/v2\/posts\/7819\/revisions\/24791"}],"wp:featuredmedia":[{"embeddable":true,"href":"https:\/\/nanovea.com\/ja\/wp-json\/wp\/v2\/media\/11695"}],"wp:attachment":[{"href":"https:\/\/nanovea.com\/ja\/wp-json\/wp\/v2\/media?parent=7819"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"https:\/\/nanovea.com\/ja\/wp-json\/wp\/v2\/categories?post=7819"},{"taxonomy":"post_tag","embeddable":true,"href":"https:\/\/nanovea.com\/ja\/wp-json\/wp\/v2\/tags?post=7819"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}