{"id":7593,"date":"2020-01-19T18:16:06","date_gmt":"2020-01-19T18:16:06","guid":{"rendered":"https:\/\/nanovea.com\/?p=7593"},"modified":"2023-11-13T22:34:06","modified_gmt":"2023-11-13T22:34:06","slug":"%e6%a5%b5%e4%bd%8e%e9%80%9f%e5%9f%9f%e3%81%a7%e3%81%ae%e6%91%a9%e6%93%a6%e8%a9%95%e4%be%a1","status":"publish","type":"post","link":"https:\/\/nanovea.com\/ja\/friction-evaluation-at-extreme-low-speeds\/","title":{"rendered":"\u6975\u4f4e\u901f\u57df\u3067\u306e\u6469\u64e6\u8a55\u4fa1"},"content":{"rendered":"<div data-elementor-type=\"wp-post\" data-elementor-id=\"7593\" class=\"elementor elementor-7593\" data-elementor-post-type=\"post\">\n\t\t\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-29bc285 elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"29bc285\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-9b35475\" data-id=\"9b35475\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<section class=\"elementor-section elementor-inner-section elementor-element elementor-element-cf7b249 elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"cf7b249\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-inner-column elementor-element elementor-element-08670eb\" data-id=\"08670eb\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-d7ff982 elementor-widget elementor-widget-spacer\" data-id=\"d7ff982\" data-element_type=\"widget\" data-widget_type=\"spacer.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t<div class=\"elementor-spacer\">\n\t\t\t<div class=\"elementor-spacer-inner\"><\/div>\n\t\t<\/div>\n\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-inner-column elementor-element elementor-element-98a0848\" data-id=\"98a0848\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-64a40e5 elementor-widget elementor-widget-html\" data-id=\"64a40e5\" data-element_type=\"widget\" data-widget_type=\"html.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<div><\/div>\r\n<a href=\"http:\/\/nanovea.com\/App-Notes\/rubber-friction-evaluation.pdf\"\" target=\"_blank\">\r\n<div class=\"product-features-icon-image-containter-brochure-button\">\r\n\r\n<img decoding=\"async\" class=\"alignright\" style=\"width: 200px;\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2020\/06\/DOWNLOAD-PDF-BUTTON-A-s.png\" \/>\r\n<div class=\"overlay-button\"><img decoding=\"async\" class=\"alignright\" style=\"width: 200px;\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2020\/06\/DOWNLOAD-PDF-BUTTON-B-s.png\" \/><\/div>\r\n<\/div>\r\n<\/a>\r\n<div>\u00a0<\/div>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-7f9aa28 elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"7f9aa28\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-7fa57f8d\" data-id=\"7fa57f8d\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-608e0728 elementor-widget elementor-widget-text-editor\" data-id=\"608e0728\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p style=\"text-align: left; color: #1b96cf; font-size: 24px;\">\u4f4e\u901f\u57df\u3067\u306e\u6469\u64e6\u8a55\u4fa1\u306e\u91cd\u8981\u6027<\/p>\n<p>\u6469\u64e6\u3068\u306f\u3001\u56fa\u4f53\u8868\u9762\u540c\u58eb\u3092\u6ed1\u3089\u305b\u3066\u76f8\u5bfe\u904b\u52d5\u306b\u62b5\u6297\u3055\u305b\u308b\u529b\u306e\u3053\u3068\u3067\u3042\u308b\u3002\u3053\u306e2\u3064\u306e\u63a5\u89e6\u9762\u306e\u76f8\u5bfe\u904b\u52d5\u304c\u8d77\u3053\u308b\u3068\u3001\u754c\u9762\u3067\u306e\u6469\u64e6\u306b\u3088\u308a\u904b\u52d5\u30a8\u30cd\u30eb\u30ae\u30fc\u304c\u71b1\u306b\u5909\u63db\u3055\u308c\u308b\u3002\u307e\u305f\u3001\u3053\u306e\u3088\u3046\u306a\u30d7\u30ed\u30bb\u30b9\u306f\u3001\u6750\u6599\u306e\u6469\u8017\u3001\u3072\u3044\u3066\u306f\u4f7f\u7528\u4e2d\u306e\u90e8\u54c1\u306e\u6027\u80fd\u52a3\u5316\u306b\u3064\u306a\u304c\u308b\u53ef\u80fd\u6027\u304c\u3042\u308b\u3002<br>\u30b4\u30e0\u306f\u4f38\u3073\u7387\u304c\u5927\u304d\u304f\u3001\u5f3e\u529b\u6027\u306b\u5bcc\u307f\u3001\u9632\u6c34\u6027\u3084\u8010\u6469\u8017\u6027\u306b\u3082\u512a\u308c\u3066\u3044\u308b\u305f\u3081\u3001\u81ea\u52d5\u8eca\u306e\u30bf\u30a4\u30e4\u3084\u30ef\u30a4\u30d1\u30fc\u30d6\u30ec\u30fc\u30c9\u3001\u9774\u5e95\u306a\u3069\u3001\u6469\u64e6\u304c\u91cd\u8981\u306a\u5f79\u5272\u3092\u679c\u305f\u3059\u3055\u307e\u3056\u307e\u306a\u7528\u9014\u3084\u88fd\u54c1\u306b\u5e45\u5e83\u304f\u4f7f\u7528\u3055\u308c\u3066\u3044\u308b\u3002\u3053\u308c\u3089\u306e\u7528\u9014\u306e\u6027\u8cea\u3084\u8981\u6c42\u306b\u5fdc\u3058\u3066\u3001\u7570\u306a\u308b\u6750\u6599\u306b\u5bfe\u3057\u3066\u9ad8\u3044\u6469\u64e6\u3068\u4f4e\u3044\u6469\u64e6\u306e\u3069\u3061\u3089\u304b\u304c\u671b\u307e\u308c\u308b\u3002\u305d\u306e\u305f\u3081\u3001\u3055\u307e\u3056\u307e\u306a\u8868\u9762\u306b\u5bfe\u3059\u308b\u30b4\u30e0\u306e\u6469\u64e6\u3092\u5236\u5fa1\u3057\u3001\u4fe1\u983c\u6027\u306e\u9ad8\u3044\u65b9\u6cd5\u3067\u6e2c\u5b9a\u3059\u308b\u3053\u3068\u304c\u91cd\u8981\u306b\u306a\u308a\u307e\u3059\u3002<\/p>\n<p><br><br><\/p>\n<p style=\"text-align: left; color: #1b96cf; font-size: 24px;\">\u6e2c\u5b9a\u76ee\u7684<\/p>\n<p>\u3055\u307e\u3056\u307e\u306a\u6750\u6599\u306b\u5bfe\u3059\u308b\u30b4\u30e0\u306e\u6469\u64e6\u4fc2\u6570 (COF) \u306f\u3001Nanovea \u3092\u4f7f\u7528\u3057\u3066\u5236\u5fa1\u304a\u3088\u3073\u76e3\u8996\u3055\u308c\u305f\u65b9\u6cd5\u3067\u6e2c\u5b9a\u3055\u308c\u307e\u3059\u3002 <a href=\"https:\/\/nanovea.com\/tribometers\/\">\u30c8\u30e9\u30a4\u30dc\u30e1\u30fc\u30bf<\/a>\u3002\u3053\u306e\u7814\u7a76\u3067\u306f\u3001\u6975\u4f4e\u901f\u3067\u3055\u307e\u3056\u307e\u306a\u6750\u6599\u306e COF \u3092\u6e2c\u5b9a\u3059\u308b Nanovea \u30c8\u30e9\u30a4\u30dc\u30e1\u30fc\u30bf\u30fc\u306e\u80fd\u529b\u3092\u7d39\u4ecb\u3057\u305f\u3044\u3068\u601d\u3044\u307e\u3059\u3002<\/p>\n<p><br><\/p>\n<p><a href=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/12\/Sample-picture-measured-compressed.png\"><img fetchpriority=\"high\" decoding=\"async\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/12\/Sample-picture-measured-compressed.png\" alt=\"\" width=\"854\" height=\"451\"><\/a><\/p>\n\n<p><br><br><\/p>\n<p style=\"text-align: left; color: #1b96cf; font-size: 24px;\">\u7d50\u679c\u304a\u3088\u3073\u8003\u5bdf<\/p>\n<p>3\u7a2e\u985e\u306e\u6750\u6599\uff08Stainless steel SS 316, Cu 110, optional Acrylic\uff09\u306b\u5bfe\u3059\u308b\u30b4\u30e0\u7403\uff08\u03c66mm, RubberMill\uff09\u306e\u6469\u64e6\u4fc2\u6570\uff08COF\uff09\u3092Nanovea Tribometer\u3067\u8a55\u4fa1\u3057\u305f\uff0e\u8a66\u9a13\u3057\u305f\u91d1\u5c5e\u30b5\u30f3\u30d7\u30eb\u306f\u3001\u6e2c\u5b9a\u524d\u306b\u6a5f\u68b0\u7684\u306b\u7814\u78e8\u3057\u3001\u93e1\u9762\u4ed5\u4e0a\u3052\u3068\u3057\u305f\u3002\u6cd5\u7dda\u8377\u91cd\u3092\u52a0\u3048\u305f\u969b\u306e\u30b4\u30e0\u7403\u306e\u308f\u305a\u304b\u306a\u5909\u5f62\u306b\u3088\u3063\u3066\u9762\u7a4d\u63a5\u89e6\u304c\u751f\u3058\u3001COF\u6e2c\u5b9a\u306b\u5bfe\u3059\u308b\u8a66\u6599\u8868\u9762\u306e\u30a2\u30b9\u30da\u30ea\u30c6\u30a3\u3084\u4e0d\u5747\u4e00\u6027\u306e\u5f71\u97ff\u3092\u8efd\u6e1b\u3059\u308b\u3053\u3068\u3082\u3067\u304d\u307e\u3059\u3002\u8a66\u9a13\u30d1\u30e9\u30e1\u30fc\u30bf\u3092\u8868 1 \u306b\u793a\u3059\u3002<\/p>\n<p><br><\/p>\n<div style=\"text-align: center;\"><a href=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/12\/Test-procedure-Rubber-friction.png\"><img decoding=\"async\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/12\/Test-procedure-Rubber-friction.png\" alt=\"\" width=\"493\" height=\"415\"><\/a><\/div>\n<div style=\"text-align: center;\">&nbsp;<\/div>\n<p>4\u7a2e\u985e\u306e\u901f\u5ea6\u3067\u7570\u306a\u308b\u7d20\u6750\u306b\u5bfe\u3057\u3066\u30b4\u30e0\u7403\u3092\u885d\u7a81\u3055\u305b\u305f\u3068\u304d\u306eCOF\u3092\u56f32\u306b\u793a\u3059\u30022 \u306b\u3001\u30bd\u30d5\u30c8\u30a6\u30a7\u30a2\u306b\u3088\u3063\u3066\u81ea\u52d5\u7684\u306b\u8a08\u7b97\u3055\u308c\u305f\u5e73\u5747 COF \u3092\u307e\u3068\u3081\u3001\u56f3 3 \u3067\u6bd4\u8f03\u3057\u305f\u3002\u8208\u5473\u6df1\u3044\u3053\u3068\u306b\u3001\u91d1\u5c5e\u8a66\u6599\uff08SS 316 \u3068 Cu 110\uff09\u306f\u3001\u56de\u8ee2\u901f\u5ea6\u304c 0.01 rpm \u3068\u3044\u3046\u975e\u5e38\u306b\u4f4e\u3044\u5024\u304b\u3089 5 rpm \u307e\u3067\u4e0a\u6607\u3059\u308b\u3068\u3001COF \u304c\u8457\u3057\u304f\u5897\u52a0\u3059\u308b\u3053\u3068\u304c\u308f\u304b\u308a\u307e\u3059\u3002\u3053\u306e\u7d50\u679c\u306f\u3001\u3044\u304f\u3064\u304b\u306e\u7814\u7a76\u5ba4\u304b\u3089\u5831\u544a\u3055\u308c\u3066\u3044\u308b\u7d50\u679c\u3068\u4e00\u81f4\u3057\u3066\u3044\u308b\u3002Grosch\u304c\u63d0\u6848\u3057\u305f\u3088\u3046\u306b<sup>4<\/sup> \u30b4\u30e0\u306e\u6469\u64e6\u306f\u3001\u4e3b\u306b\uff081\uff09\u30b4\u30e0\u3068\u4ed6\u306e\u6750\u6599\u306e\u63a5\u7740\u3001\uff082\uff09\u8868\u9762\u306e\u51f9\u51f8\u306b\u3088\u308b\u30b4\u30e0\u306e\u5909\u5f62\u306b\u3088\u308b\u30a8\u30cd\u30eb\u30ae\u30fc\u640d\u5931\u306e2\u3064\u306e\u30e1\u30ab\u30cb\u30ba\u30e0\u3067\u6c7a\u5b9a\u3055\u308c\u308b\u3002\u30b7\u30e3\u30e9\u30de\u30c3\u30cf<sup>5<\/sup> \u8edf\u8cea\u30b4\u30e0\u7403\u3068\u786c\u8cea\u8868\u9762\u3068\u306e\u754c\u9762\u306b\u304a\u3044\u3066\uff0c\u30b4\u30e0\u304c\u76f8\u624b\u6750\u304b\u3089\u5265\u96e2\u3059\u308b\u6ce2\u304c\u89b3\u5bdf\u3055\u308c\u305f\u3002\u30b4\u30e0\u304c\u57fa\u6750\u8868\u9762\u304b\u3089\u5265\u96e2\u3059\u308b\u529b\u3068\u5265\u96e2\u306e\u6ce2\u306e\u901f\u5ea6\u304b\u3089\u3001\u8a66\u9a13\u4e2d\u306e\u7570\u306a\u308b\u901f\u5ea6\u3067\u306e\u6469\u64e6\u306e\u9055\u3044\u3092\u8aac\u660e\u3059\u308b\u3053\u3068\u304c\u3067\u304d\u308b\u3002<\/p>\n<p>\u3053\u308c\u306b\u5bfe\u3057\u3001\u30b4\u30e0\u3068\u30a2\u30af\u30ea\u30eb\u306e\u30ab\u30c3\u30d7\u30eb\u306f\u3001\u7570\u306a\u308b\u56de\u8ee2\u6570\u3067\u9ad8\u3044COF\u3092\u793a\u3057\u307e\u3057\u305f\u3002\u56de\u8ee2\u901f\u5ea6\u304c0.01 rpm\u304b\u30895 rpm\u307e\u3067\u4e0a\u6607\u3059\u308b\u3068\u3001COF\u5024\u306f1.02\u304b\u30891.09\u307e\u3067\u308f\u305a\u304b\u306b\u4e0a\u6607\u3057\u305f\u3002\u3053\u306e\u3088\u3046\u306a\u9ad8\u3044COF\u306f\u3001\u304a\u305d\u3089\u304f\u8a66\u9a13\u4e2d\u306b\u5f62\u6210\u3055\u308c\u305f\u63a5\u89e6\u9762\u306e\u5c40\u6240\u7684\u306a\u5316\u5b66\u7d50\u5408\u304c\u5f37\u304f\u306a\u3063\u305f\u3053\u3068\u306b\u8d77\u56e0\u3057\u3066\u3044\u307e\u3059\u3002<\/p>\n\n<p><br><br><\/p>\n<div style=\"float: left;\"><a href=\"https:\/\/nanovea.com\/wp-content\/uploads\/2019\/12\/figure-1.png\"><img decoding=\"async\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2019\/12\/figure-1.png\" alt=\"\" width=\"356\" height=\"527\"><\/a><\/div>\n<div style=\"float: right;\"><a href=\"https:\/\/nanovea.com\/wp-content\/uploads\/2019\/12\/figure-2.png\"><img loading=\"lazy\" decoding=\"async\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2019\/12\/figure-2.png\" alt=\"\" width=\"344\" height=\"527\"><\/a><\/div>\n<div style=\"text-align: center;\">&nbsp;<\/div>\n<div style=\"display: inline-block; padding-top: 4%;\">&nbsp;<\/div>\n<p><strong><u><i>&nbsp;<\/i><\/u><\/strong><\/p>\n<p><strong><u><i>&nbsp;<\/i><\/u><\/strong><\/p>\n\n<p><br><br><br><\/p>\n<p style=\"text-align: left; color: #1b96cf; font-size: 24px;\">\u7d50\u8ad6<\/p>\n<p><br><\/p>\n<div style=\"text-align: center;\"><a href=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/12\/eraser-conclusion-photo.png\"><img loading=\"lazy\" decoding=\"async\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/12\/eraser-conclusion-photo.png\" alt=\"\" width=\"788\" height=\"312\"><\/a><\/div>\n<p><br><\/p>\n<p>\u672c\u7814\u7a76\u3067\u306f\u3001\u30b4\u30e0\u304c\u6975\u4f4e\u901f\u3067\u3001\u786c\u3044\u8868\u9762\u306b\u5bfe\u3059\u308b\u6469\u64e6\u304c\u76f8\u5bfe\u904b\u52d5\u306e\u901f\u5ea6\u304c\u4e0a\u304c\u308b\u306b\u3064\u308c\u3066\u5927\u304d\u304f\u306a\u308b\u3068\u3044\u3046\u7279\u7570\u306a\u6469\u64e6\u6319\u52d5\u3092\u793a\u3059\u3053\u3068\u3092\u793a\u3057\u305f\u3002\u30b4\u30e0\u306f\u3001\u7570\u306a\u308b\u6750\u6599\u306e\u4e0a\u3092\u6ed1\u308b\u3068\u304d\u3001\u7570\u306a\u308b\u6469\u64e6\u3092\u793a\u3057\u307e\u3059\u3002\u30ca\u30ce\u30d9\u30fc\u30b9\u30c8\u30e9\u30a4\u30dc\u30e1\u30fc\u30bf\u306f\u3001\u7570\u306a\u308b\u901f\u5ea6\u3067\u5236\u5fa1\u30fb\u76e3\u8996\u3055\u308c\u305f\u65b9\u6cd5\u3067\u6750\u6599\u306e\u6469\u64e6\u7279\u6027\u3092\u8a55\u4fa1\u3059\u308b\u3053\u3068\u304c\u3067\u304d\u3001\u30e6\u30fc\u30b6\u30fc\u306f\u6750\u6599\u306e\u6469\u64e6\u30e1\u30ab\u30cb\u30ba\u30e0\u306e\u57fa\u672c\u7684\u306a\u7406\u89e3\u3092\u6df1\u3081\u3001\u76ee\u6a19\u3068\u3059\u308b\u30c8\u30e9\u30a4\u30dc\u30ed\u30b8\u30fc\u5de5\u5b66\u30a2\u30d7\u30ea\u30b1\u30fc\u30b7\u30e7\u30f3\u306b\u6700\u9069\u306a\u6750\u6599\u30ab\u30c3\u30d7\u30eb\u3092\u9078\u629e\u3059\u308b\u3053\u3068\u304c\u53ef\u80fd\u3067\u3059\u3002<\/p>\n<p>\u30ca\u30ce\u30d9\u30fc\u30b9\u30c8\u30e9\u30a4\u30dc\u30e1\u30fc\u30bf\u306f\u3001ISO\u304a\u3088\u3073ASTM\u306b\u6e96\u62e0\u3057\u305f\u56de\u8ee2\u30e2\u30fc\u30c9\u3068\u30ea\u30cb\u30a2\u30e2\u30fc\u30c9\u306b\u3088\u308b\u7cbe\u5bc6\u3067\u518d\u73fe\u6027\u306e\u9ad8\u3044\u6469\u8017\u30fb\u6469\u64e6\u8a66\u9a13\u3068\u3001\u30aa\u30d7\u30b7\u30e7\u30f3\u3067\u9ad8\u6e29\u6469\u8017\u3001\u6f64\u6ed1\u3001\u30c8\u30e9\u30a4\u30dc\u30b3\u30ed\u30fc\u30b8\u30e7\u30f3\u30921\u3064\u306e\u7d71\u5408\u3055\u308c\u305f\u30b7\u30b9\u30c6\u30e0\u3067\u5229\u7528\u3059\u308b\u3053\u3068\u304c\u53ef\u80fd\u3067\u3059\u30020.01 rpm\u307e\u3067\u306e\u6975\u3081\u3066\u4f4e\u3044\u901f\u5ea6\u3067\u56de\u8ee2\u30b9\u30c6\u30fc\u30b8\u3092\u5236\u5fa1\u3057\u3001\u6469\u64e6\u306e\u5909\u5316\u3092\u305d\u306e\u5834\u3067\u30e2\u30cb\u30bf\u30fc\u3059\u308b\u3053\u3068\u304c\u53ef\u80fd\u3067\u3059\u3002\u30ca\u30ce\u30d9\u30a2\u306e\u6bd4\u985e\u306a\u304d\u88fd\u54c1\u7fa4\u306f\u3001\u8584\u3044\u307e\u305f\u306f\u539a\u3044\u3001\u67d4\u3089\u304b\u3044\u307e\u305f\u306f\u786c\u3044\u30b3\u30fc\u30c6\u30a3\u30f3\u30b0\u3001\u30d5\u30a3\u30eb\u30e0\u3001\u304a\u3088\u3073\u57fa\u6750\u306e\u30c8\u30e9\u30a4\u30dc\u30ed\u30b8\u30fc\u7279\u6027\u3092\u30d5\u30eb\u30ec\u30f3\u30b8\u3067\u6e2c\u5b9a\u3059\u308b\u305f\u3081\u306e\u7406\u60f3\u7684\u306a\u30bd\u30ea\u30e5\u30fc\u30b7\u30e7\u30f3\u3068\u306a\u308a\u307e\u3059\u3002<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-99195ac elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"99195ac\" data-element_type=\"section\" data-settings=\"{&quot;background_background&quot;:&quot;classic&quot;}\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-7c65b15\" data-id=\"7c65b15\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-62764f0 elementor-widget elementor-widget-heading\" data-id=\"62764f0\" data-element_type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\"><b>\u3055\u3066\u3001\u6b21\u306f\u30a2\u30d7\u30ea\u30b1\u30fc\u30b7\u30e7\u30f3\u306b\u3064\u3044\u3066\u3067\u3059\u3002<\/b><\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-ab334d6 live-chat elementor-align-center elementor-widget elementor-widget-button\" data-id=\"ab334d6\" data-element_type=\"widget\" data-widget_type=\"button.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<div class=\"elementor-button-wrapper\">\n\t\t\t\t\t<a class=\"elementor-button elementor-button-link elementor-size-md\" href=\"https:\/\/nanovea.com\/contact\/live-chat\/\" id=\"live-chat\">\n\t\t\t\t\t\t<span class=\"elementor-button-content-wrapper\">\n\t\t\t\t\t\t\t\t\t<span class=\"elementor-button-text\">\u30e9\u30a4\u30d6\u30c1\u30e3\u30c3\u30c8<\/span>\n\t\t\t\t\t<\/span>\n\t\t\t\t\t<\/a>\n\t\t\t\t<\/div>\n\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<\/div>","protected":false},"excerpt":{"rendered":"","protected":false},"author":1,"featured_media":11710,"comment_status":"open","ping_status":"open","sticky":false,"template":"","format":"standard","meta":{"_exactmetrics_skip_tracking":false,"_exactmetrics_sitenote_active":false,"_exactmetrics_sitenote_note":"","_exactmetrics_sitenote_category":0,"footnotes":""},"categories":[7,348,349,337,373,336],"tags":[],"class_list":["post-7593","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-application-notes","category-friction-testing-coefficient-of-friction","category-laboratory-testing","category-mechanical-testing","category-rotational-tribology","category-tribology-testing"],"_links":{"self":[{"href":"https:\/\/nanovea.com\/ja\/wp-json\/wp\/v2\/posts\/7593","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/nanovea.com\/ja\/wp-json\/wp\/v2\/posts"}],"about":[{"href":"https:\/\/nanovea.com\/ja\/wp-json\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"https:\/\/nanovea.com\/ja\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/nanovea.com\/ja\/wp-json\/wp\/v2\/comments?post=7593"}],"version-history":[{"count":60,"href":"https:\/\/nanovea.com\/ja\/wp-json\/wp\/v2\/posts\/7593\/revisions"}],"predecessor-version":[{"id":23423,"href":"https:\/\/nanovea.com\/ja\/wp-json\/wp\/v2\/posts\/7593\/revisions\/23423"}],"wp:featuredmedia":[{"embeddable":true,"href":"https:\/\/nanovea.com\/ja\/wp-json\/wp\/v2\/media\/11710"}],"wp:attachment":[{"href":"https:\/\/nanovea.com\/ja\/wp-json\/wp\/v2\/media?parent=7593"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"https:\/\/nanovea.com\/ja\/wp-json\/wp\/v2\/categories?post=7593"},{"taxonomy":"post_tag","embeddable":true,"href":"https:\/\/nanovea.com\/ja\/wp-json\/wp\/v2\/tags?post=7593"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}