{"id":11395,"date":"2021-05-13T19:40:10","date_gmt":"2021-05-13T19:40:10","guid":{"rendered":"https:\/\/nanovea.com\/?p=11395"},"modified":"2025-05-22T20:41:51","modified_gmt":"2025-05-22T20:41:51","slug":"%e3%82%ac%e3%83%a9%e3%82%b9%e3%82%b3%e3%83%bc%e3%83%86%e3%82%a3%e3%83%b3%e3%82%b0%e3%81%ae%e8%80%90%e6%b9%bf%e6%80%a7%e8%a9%a6%e9%a8%93%ef%bc%88%e3%83%88%e3%83%a9%e3%82%a4%e3%83%9c%e3%83%a1%e3%83%bc","status":"publish","type":"post","link":"https:\/\/nanovea.com\/ja\/glass-coating-humidity-wear-testing-by-tribometer\/","title":{"rendered":"\u30c8\u30e9\u30a4\u30dc\u30e1\u30fc\u30bf\u306b\u3088\u308b\u30ac\u30e9\u30b9\u88ab\u819c\u306e\u8010\u6e7f\u6027\u8a66\u9a13"},"content":{"rendered":"<div data-elementor-type=\"wp-post\" data-elementor-id=\"11395\" class=\"elementor elementor-11395\" data-elementor-post-type=\"post\">\n\t\t\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-665ca0e elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"665ca0e\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-153f3ac\" data-id=\"153f3ac\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-fc48c11 elementor-widget elementor-widget-text-editor\" data-id=\"fc48c11\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p>\u30c8\u30e9\u30a4\u30dc\u30e1\u30fc\u30bf\u306b\u3088\u308b\u30ac\u30e9\u30b9\u88ab\u819c\u306e\u8010\u6e7f\u6027\u8a66\u9a13<\/p><p>\u8a73\u7d30\u306f\u3053\u3061\u3089<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-7ec3d48 elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"7ec3d48\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-c477953\" data-id=\"c477953\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-cec2c6e elementor-widget elementor-widget-heading\" data-id=\"cec2c6e\" data-element_type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\"><span>\u30ac\u30e9\u30b9\u30b3\u30fc\u30c8\u6e7f\u5ea6<\/span><\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-d107f9b elementor-widget elementor-widget-heading\" data-id=\"d107f9b\" data-element_type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\"><span>\u30c8\u30e9\u30a4\u30dc\u30e1\u30fc\u30bf\u306b\u3088\u308b\u6469\u8017\u8a66\u9a13<\/span><\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-73c118d elementor-widget elementor-widget-image\" data-id=\"73c118d\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img fetchpriority=\"high\" decoding=\"async\" width=\"1024\" height=\"290\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2021\/05\/Glass-Coating-Humidity-Test-Skyscraper.png\" class=\"attachment-large size-large wp-image-11402\" alt=\"\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-97cc106 elementor-widget elementor-widget-heading\" data-id=\"97cc106\" data-element_type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\">\u4f5c\u6210\u8005<\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-95aa94e elementor-widget elementor-widget-heading\" data-id=\"95aa94e\" data-element_type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\"><span>DUANJIE LI<\/span><span style=\"font-size:17pt\">\u535a\u58eb\u53f7\u53d6\u5f97 <\/span><span><\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-0d45a0f elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"0d45a0f\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-184b495\" data-id=\"184b495\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-24a6026 elementor-widget elementor-widget-spacer\" data-id=\"24a6026\" data-element_type=\"widget\" data-widget_type=\"spacer.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t<div class=\"elementor-spacer\">\n\t\t\t<div class=\"elementor-spacer-inner\"><\/div>\n\t\t<\/div>\n\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-753c1f3 elementor-section-content-middle elementor-reverse-mobile elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"753c1f3\" data-element_type=\"section\" data-settings=\"{&quot;background_background&quot;:&quot;classic&quot;}\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-top-column elementor-element elementor-element-f2074e4\" data-id=\"f2074e4\" data-element_type=\"column\" data-settings=\"{&quot;background_background&quot;:&quot;classic&quot;}\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-c53ea2a elementor-widget elementor-widget-spacer\" data-id=\"c53ea2a\" data-element_type=\"widget\" data-widget_type=\"spacer.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t<div class=\"elementor-spacer\">\n\t\t\t<div class=\"elementor-spacer-inner\"><\/div>\n\t\t<\/div>\n\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-top-column elementor-element elementor-element-b259d86\" data-id=\"b259d86\" data-element_type=\"column\" data-settings=\"{&quot;background_background&quot;:&quot;classic&quot;}\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-62f2a44 elementor-widget elementor-widget-heading\" data-id=\"62f2a44\" data-element_type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\">\u306f\u3058\u3081\u306b<\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-9ab0009 elementor-widget elementor-widget-text-editor\" data-id=\"9ab0009\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p><span class=\"fontstyle0\">\u30bb\u30eb\u30d5\u30af\u30ea\u30fc\u30cb\u30f3\u30b0\u6a5f\u80fd\u4ed8\u304d\u30ac\u30e9\u30b9\u30b3\u30fc\u30c6\u30a3\u30f3\u30b0\u306f\u3001\u6c5a\u308c\u3001\u57a2\u3001\u30b7\u30df\u306e\u84c4\u7a4d\u3092\u9632\u304e\u3001\u6e05\u6383\u3057\u3084\u3059\u3044\u30ac\u30e9\u30b9\u8868\u9762\u3092\u4f5c\u308a\u51fa\u3057\u307e\u3059\u3002\u305d\u306e\u30bb\u30eb\u30d5\u30af\u30ea\u30fc\u30cb\u30f3\u30b0\u6a5f\u80fd\u306f\u3001\u6e05\u6383\u983b\u5ea6\u3001\u6642\u9593\u3001\u30a8\u30cd\u30eb\u30ae\u30fc\u3001\u6e05\u6383\u30b3\u30b9\u30c8\u3092\u5927\u5e45\u306b\u524a\u6e1b\u3057\u3001\u30ac\u30e9\u30b9\u30d5\u30a1\u30b5\u30fc\u30c9\u3001\u93e1\u3001\u30b7\u30e3\u30ef\u30fc\u30ac\u30e9\u30b9\u3001\u7a93\u3001\u30d5\u30ed\u30f3\u30c8\u30ac\u30e9\u30b9\u306a\u3069\u3001\u4f4f\u5b85\u3084\u5546\u696d\u306e\u3055\u307e\u3056\u307e\u306a\u7528\u9014\u306b\u9b45\u529b\u7684\u306a\u9078\u629e\u80a2\u3092\u63d0\u4f9b\u3057\u307e\u3059\u3002<\/span><\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-c9a07fb elementor-widget elementor-widget-heading\" data-id=\"c9a07fb\" data-element_type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\">\u8010\u6469\u8017\u6027\u306e\u91cd\u8981\u6027\n\u30bb\u30eb\u30d5\u30af\u30ea\u30fc\u30cb\u30f3\u30b0\u30ac\u30e9\u30b9\u30b3\u30fc\u30c6\u30a3\u30f3\u30b0\u306e<\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-e74abb9 elementor-widget elementor-widget-text-editor\" data-id=\"e74abb9\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p><span class=\"fontstyle0\">\u30bb\u30eb\u30d5\u30af\u30ea\u30fc\u30cb\u30f3\u30b0\u30b3\u30fc\u30c6\u30a3\u30f3\u30b0\u306e\u4e3b\u306a\u7528\u9014\u306f\u3001\u8d85\u9ad8\u5c64\u30d3\u30eb\u306e\u30ac\u30e9\u30b9\u30d5\u30a1\u30b5\u30fc\u30c9\u306e\u5916\u9762\u3067\u3042\u308b\u3002\u30ac\u30e9\u30b9\u8868\u9762\u306f\u3001\u5f37\u98a8\u306b\u3088\u3063\u3066\u904b\u3070\u308c\u3066\u304f\u308b\u9ad8\u901f\u306e\u7c92\u5b50\u306b\u3088\u3063\u3066\u3057\u3070\u3057\u3070\u653b\u6483\u3055\u308c\u308b\u3002\u307e\u305f\u3001\u5929\u5019\u3082\u30ac\u30e9\u30b9\u30b3\u30fc\u30c6\u30a3\u30f3\u30b0\u306e\u8010\u7528\u5e74\u6570\u306b\u5927\u304d\u306a\u5f71\u97ff\u3092\u4e0e\u3048\u307e\u3059\u3002\u30ac\u30e9\u30b9\u304c\u52a3\u5316\u3057\u305f\u5834\u5408\u3001\u8868\u9762\u51e6\u7406\u3092\u65bd\u3057\u3001\u65b0\u3057\u3044\u30b3\u30fc\u30c6\u30a3\u30f3\u30b0\u3092\u65bd\u3059\u3053\u3068\u306f\u975e\u5e38\u306b\u56f0\u96e3\u3067\u3042\u308a\u3001\u30b3\u30b9\u30c8\u3082\u304b\u304b\u308b\u3002\u305d\u306e\u305f\u3081\u3001\u30ac\u30e9\u30b9\u30b3\u30fc\u30c6\u30a3\u30f3\u30b0\u306e\u8010\u6469\u8017\u6027\u306b\u306f\u3001\u5929\u5019\u306b\u5de6\u53f3\u3055\u308c\u306a\u3044\u3053\u3068\u304c\u91cd\u8981\u3067\u3059\u3002<br \/>\u5929\u5019\u306e\u5909\u5316\u304c\u91cd\u8981\u3067\u3059\u3002<\/span><\/p><p><span class=\"fontstyle0\"><br \/>\u7570\u306a\u308b\u5929\u5019\u4e0b\u3067\u306e\u30bb\u30eb\u30d5\u30af\u30ea\u30fc\u30cb\u30f3\u30b0\u30b3\u30fc\u30c6\u30a3\u30f3\u30b0\u306e\u73fe\u5b9f\u7684\u306a\u74b0\u5883\u6761\u4ef6\u3092\u30b7\u30df\u30e5\u30ec\u30fc\u30c8\u3059\u308b\u305f\u3081\u306b\u306f\u3001\u6e7f\u5ea6\u3092\u5236\u5fa1\u30fb\u76e3\u8996\u3057\u305f\u72b6\u614b\u3067\u306e\u518d\u73fe\u6027\u306e\u3042\u308b\u6469\u8017\u8a55\u4fa1\u304c\u5fc5\u8981\u3067\u3059\u3002\u3053\u308c\u306b\u3088\u308a\u3001\u30e6\u30fc\u30b6\u30fc\u306f\u7570\u306a\u308b\u6e7f\u5ea6\u306b\u3055\u3089\u3055\u308c\u305f\u30bb\u30eb\u30d5\u30af\u30ea\u30fc\u30cb\u30f3\u30b0\u30b3\u30fc\u30c6\u30a3\u30f3\u30b0\u306e\u8010\u6469\u8017\u6027\u3092\u9069\u5207\u306b\u6bd4\u8f03\u3057\u3001\u76ee\u6a19\u3068\u3059\u308b\u30a2\u30d7\u30ea\u30b1\u30fc\u30b7\u30e7\u30f3\u306b\u6700\u9069\u306a\u5019\u88dc\u3092\u9078\u629e\u3059\u308b\u3053\u3068\u304c\u3067\u304d\u307e\u3059\u3002<\/span> <\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-bbe0c25 elementor-reverse-mobile elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"bbe0c25\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-5bda47b\" data-id=\"5bda47b\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<section class=\"elementor-section elementor-inner-section elementor-element elementor-element-5986dd7 elementor-reverse-mobile elementor-section-full_width elementor-reverse-tablet elementor-section-height-default elementor-section-height-default\" data-id=\"5986dd7\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-no\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-inner-column elementor-element elementor-element-77e62ae\" data-id=\"77e62ae\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-ae83510 elementor-widget elementor-widget-text-editor\" data-id=\"ae83510\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p>\u6e2c\u5b9a\u76ee\u7684<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-5556e11 elementor-widget elementor-widget-text-editor\" data-id=\"5556e11\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p><em><span class=\"fontstyle0\">\u3053\u306e\u7814\u7a76\u3067\u3001\u79c1\u305f\u3061\u306f\u4ee5\u4e0b\u306e\u3053\u3068\u3092\u793a\u3057\u307e\u3057\u305f\u3002 <\/span><span class=\"fontstyle2\">\u30ca\u30ce\u30d3\u30a2 <\/span><span class=\"fontstyle0\">\u6e7f\u5ea6\u30b3\u30f3\u30c8\u30ed\u30fc\u30e9\u3092\u642d\u8f09\u3057\u305fT100\u30c8\u30e9\u30a4\u30dc\u30e1\u30fc\u30bf\u306f\u3001\u7570\u306a\u308b\u6e7f\u5ea6\u74b0\u5883\u306b\u304a\u3051\u308b\u30bb\u30eb\u30d5\u30af\u30ea\u30fc\u30cb\u30f3\u30b0\u30ac\u30e9\u30b9\u30b3\u30fc\u30c6\u30a3\u30f3\u30b0\u306e\u8010\u6469\u8017\u6027\u3092\u8abf\u67fb\u3059\u308b\u305f\u3081\u306e\u7406\u60f3\u7684\u306a\u30c4\u30fc\u30eb\u3067\u3059\u3002<\/span><\/em><\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-34fc6f9 elementor-widget elementor-widget-spacer\" data-id=\"34fc6f9\" data-element_type=\"widget\" data-widget_type=\"spacer.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t<div class=\"elementor-spacer\">\n\t\t\t<div class=\"elementor-spacer-inner\"><\/div>\n\t\t<\/div>\n\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-7429702 elementor-widget elementor-widget-text-editor\" data-id=\"7429702\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p>\u30ca\u30ce\u30d3\u30a2<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-fda08d7 elementor-widget elementor-widget-text-editor\" data-id=\"fda08d7\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p>T100<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-inner-column elementor-element elementor-element-a6b67e5\" data-id=\"a6b67e5\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-911a059 elementor-widget elementor-widget-image\" data-id=\"911a059\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<a href=\"https:\/\/nanovea.com\/instruments\/t100-the-benchmark-tribometer\/\">\n\t\t\t\t\t\t\t<img decoding=\"async\" width=\"870\" height=\"800\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2020\/12\/Nanovea-T100-Benchtop-Tribometer.png\" class=\"elementor-animation-grow attachment-large size-large wp-image-9903\" alt=\"\u5c0f\u578b\u7a7a\u6c17\u5727\u5f0f\u30c8\u30e9\u30a4\u30dc\u30e1\u30fc\u30bf T100\" \/>\t\t\t\t\t\t\t\t<\/a>\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-8ec771e elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"8ec771e\" data-element_type=\"section\" data-settings=\"{&quot;background_background&quot;:&quot;classic&quot;}\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-4eba72c\" data-id=\"4eba72c\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-fbdd647 elementor-widget elementor-widget-text-editor\" data-id=\"fbdd647\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p>\u8a66\u9a13\u65b9\u6cd5<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-21f4edc elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"21f4edc\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-fbf6d1c\" data-id=\"fbf6d1c\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-ffed5c4 elementor-widget elementor-widget-text-editor\" data-id=\"ffed5c4\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p><span class=\"fontstyle0\">\u30bd\u30fc\u30c0\u30e9\u30a4\u30e0\u30ac\u30e9\u30b9\u306e\u9855\u5fae\u93e1\u30b9\u30e9\u30a4\u30c9\u306b\u30012\u7a2e\u985e\u306e\u51e6\u7406\u30ec\u30b7\u30d4\u3067\u30bb\u30eb\u30d5\u30af\u30ea\u30fc\u30f3\u30ac\u30e9\u30b9\u30b3\u30fc\u30c6\u30a3\u30f3\u30b0\u3092\u65bd\u3057\u305f\u3002\u3053\u306e2\u3064\u306e\u30b3\u30fc\u30c6\u30a3\u30f3\u30b0\u306f\u3001\u30b3\u30fc\u30c6\u30a3\u30f3\u30b01\u304a\u3088\u3073\u30b3\u30fc\u30c6\u30a3\u30f3\u30b02\u3068\u3057\u3066\u8b58\u5225\u3055\u308c\u307e\u3059\u3002\u6bd4\u8f03\u306e\u305f\u3081\u3001\u30b3\u30fc\u30c6\u30a3\u30f3\u30b0\u3055\u308c\u3066\u3044\u306a\u3044\u88f8\u306e\u30b9\u30e9\u30a4\u30c9\u30ac\u30e9\u30b9\u3082\u30c6\u30b9\u30c8\u3055\u308c\u3066\u3044\u307e\u3059\u3002<\/span><\/p><p><span class=\"fontstyle0\"><br \/><\/span><span class=\"fontstyle2\">\u30ca\u30ce\u30d3\u30a2 <\/span><span class=\"fontstyle0\"><a href=\"https:\/\/nanovea.com\/tribometers\/\">\u30c8\u30e9\u30a4\u30dc\u30e1\u30fc\u30bf <\/a>\u6e7f\u5ea6\u5236\u5fa1\u30e2\u30b8\u30e5\u30fc\u30eb\u3092\u5099\u3048\u305f\u30b7\u30b9\u30c6\u30e0\u306f\u3001\u30bb\u30eb\u30d5\u30af\u30ea\u30fc\u30f3\u30ac\u30e9\u30b9\u30b3\u30fc\u30c6\u30a3\u30f3\u30b0\u306e\u6469\u64e6\u4fc2\u6570\u3001COF\u3001\u8010\u6469\u8017\u6027\u306a\u3069\u306e\u30c8\u30e9\u30a4\u30dc\u30ed\u30b8\u30fc\u6319\u52d5\u3092\u8a55\u4fa1\u3059\u308b\u305f\u3081\u306b\u4f7f\u7528\u3055\u308c\u307e\u3057\u305f\u3002 WC \u30dc\u30fc\u30eb\u30c1\u30c3\u30d7 (\u76f4\u5f84 6 mm) \u3092\u8a66\u9a13\u30b5\u30f3\u30d7\u30eb\u306b\u5f53\u3066\u307e\u3057\u305f\u3002 COF \u306f\u305d\u306e\u5834\u3067\u8a18\u9332\u3055\u308c\u307e\u3057\u305f\u3002\u30c8\u30e9\u30a4\u30dc\u30c1\u30e3\u30f3\u30d0\u30fc\u306b\u53d6\u308a\u4ed8\u3051\u3089\u308c\u305f\u6e7f\u5ea6\u30b3\u30f3\u30c8\u30ed\u30fc\u30e9\u30fc\u306f\u3001\u76f8\u5bfe\u6e7f\u5ea6 (RH) \u5024\u3092 \u00b11 % \u306e\u7bc4\u56f2\u3067\u6b63\u78ba\u306b\u5236\u5fa1\u3057\u307e\u3057\u305f\u3002\u6469\u8017\u8a66\u9a13\u5f8c\u3001\u6469\u8017\u75d5\u306e\u5f62\u614b\u3092\u5149\u5b66\u9855\u5fae\u93e1\u3067\u691c\u67fb\u3057\u307e\u3057\u305f\u3002<\/span><\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-e589df4 elementor-widget elementor-widget-text-editor\" data-id=\"e589df4\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<span class=\"fontstyle0\" style=\"color: #000000;\">\u6700\u5927\u8377\u91cd <\/span><span class=\"fontstyle0\" style=\"color: #1b96cf;\"> <space> <space> <space> <space> 40 mN <\/span>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-3fe3f47 elementor-widget elementor-widget-image\" data-id=\"3fe3f47\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img decoding=\"async\" width=\"1024\" height=\"319\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2021\/05\/Glass-Coating-Humidity-Coefficient-of-Friction-Test.png\" class=\"attachment-large size-large wp-image-11397\" alt=\"\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-fe841c6 elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"fe841c6\" data-element_type=\"section\" data-settings=\"{&quot;background_background&quot;:&quot;classic&quot;}\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-b7a4564\" data-id=\"b7a4564\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-47cc7e1 elementor-widget elementor-widget-text-editor\" data-id=\"47cc7e1\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\u7d50\u679c\u30fb\u8003\u5bdf\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-5f29398 elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"5f29398\" data-element_type=\"section\" data-settings=\"{&quot;background_background&quot;:&quot;classic&quot;}\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-5b1376a\" data-id=\"5b1376a\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-eca2e19 elementor-widget elementor-widget-text-editor\" data-id=\"eca2e19\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p><span class=\"fontstyle0\">\u30b3\u30fc\u30c6\u30a3\u30f3\u30b0\u3055\u308c\u305f\u30ac\u30e9\u30b9\u3068\u30b3\u30fc\u30c6\u30a3\u30f3\u30b0\u3055\u308c\u3066\u3044\u306a\u3044\u30ac\u30e9\u30b9\u3067\u3001\u7570\u306a\u308b\u6e7f\u5ea6\u6761\u4ef6\u3067\u306e\u30d4\u30f3\u30aa\u30f3\u30c7\u30a3\u30b9\u30af\u6469\u8017\u8a66\u9a13\u3092\u884c\u3044\u307e\u3057\u305f<br \/>\u306e\u8a66\u6599\u3092\u7528\u3044\u305f\u3002\u306b\u793a\u3059\u3088\u3046\u306b\uff0c\u6469\u8017\u8a66\u9a13\u4e2d\u306bCOF\u3092\u305d\u306e\u5834\u3067\u8a18\u9332\u3057\u305f\u3002 <\/span><span class=\"fontstyle2\">\u56f31 <\/span><span class=\"fontstyle0\">\u3067\u3001\u5e73\u5747COF\u306f\u4ee5\u4e0b\u306e\u3088\u3046\u306b\u307e\u3068\u3081\u3089\u308c\u3066\u3044\u308b\u3002 <\/span><span class=\"fontstyle2\">\u56f32<\/span><span class=\"fontstyle0\">. <\/span><span class=\"fontstyle2\">\u56f34 <\/span><span class=\"fontstyle0\">\u306f\u3001\u6469\u8017\u8a66\u9a13\u5f8c\u306e\u6469\u8017\u75d5\u3092\u6bd4\u8f03\u3057\u307e\u3059\u3002<\/span><\/p><p><span class=\"fontstyle0\"><br \/>\u306b\u793a\u3059\u3088\u3046\u306b <\/span><span class=\"fontstyle2\">\u56f31<\/span><span class=\"fontstyle0\">30% RH\u3067\u306f\uff0c\u975e\u30b3\u30fc\u30c6\u30a3\u30f3\u30b0\u30ac\u30e9\u30b9\u306eCOF\u304c0.45\u3068\u9ad8\u304f\uff0c300\u56de\u8ee2\u306e\u6469\u8017\u8a66\u9a13\u7d42\u4e86\u6642\u306b\u306f0.6\u307e\u3067\u4e0a\u6607\u3059\u308b\uff0e\u3053\u308c\u306b\u5bfe\u3057<br \/>\u30b3\u30fc\u30c6\u30a3\u30f3\u30b0\u3055\u308c\u305f\u30ac\u30e9\u30b9\u8a66\u6599 Coating 1 \u3068 Coating 2 \u306f\uff0c\u8a66\u9a13\u958b\u59cb\u6642\u306b 0.2 \u3092\u4e0b\u56de\u308b\u4f4e\u3044 COF \u3092\u793a\u3057\u3066\u3044\u308b\u3002\u307e\u305f\u3001COF<br \/>\u306eCOF\u306f0.25\u3067\u5b89\u5b9a\u3059\u308b\u304c\u3001Coating 1\u306f0.25\u3067\u6025\u6fc0\u306b\u5897\u52a0\u3059\u308b\u3002<br \/>~250\u56de\u8ee2\u3067COF\u306f~0.5\u3068\u306a\u308b\u300260% RH\u3067\u6469\u8017\u8a66\u9a13\u3092\u5b9f\u65bd\u3059\u308b\u3068<br \/>\u975e\u30b3\u30fc\u30c6\u30a3\u30f3\u30b0\u306e\u30ac\u30e9\u30b9\u306f\u3001\u6469\u8017\u8a66\u9a13\u4e2d\u3001\u4f9d\u7136\u3068\u3057\u30660.45\u7a0b\u5ea6\u306e\u9ad8\u3044COF\u3092\u793a\u3057\u305f\u3002\u30b3\u30fc\u30c6\u30a3\u30f3\u30b0 1 \u3068 2 \u306f\u3001\u305d\u308c\u305e\u308c 0.27 \u3068 0.22 \u306e COF \u5024\u3092\u793a\u3057\u307e\u3057\u305f\u300290% RH\u3067\u306f\u3001\u975e\u30b3\u30fc\u30c6\u30a3\u30f3\u30b0\u30ac\u30e9\u30b9\u306f\u6469\u8017\u8a66\u9a13\u7d42\u4e86\u6642\u306b\u301c0.5\u3068\u3044\u3046\u9ad8\u3044COF\u3092\u6709\u3057\u3066\u3044\u307e\u3059\u3002\u30b3\u30fc\u30c6\u30a3\u30f3\u30b01\u30682\u306f\uff0c\u6469\u8017\u8a66\u9a13\u958b\u59cb\u6642\u306b\u540c\u7a0b\u5ea6\u306eCOF\uff08\u301c0.1\uff09\u3092\u793a\u3057\u3066\u3044\u308b\u3002\u30b3\u30fc\u30c6\u30a3\u30f3\u30b01\u306f\u6bd4\u8f03\u7684\u5b89\u5b9a\u3057\u305fCOF\u301c0.15\u3092\u7dad\u6301\u3057\u3066\u3044\u308b\u3002\u3057\u304b\u3057\u3001\u30b3\u30fc\u30c6\u30a3\u30f3\u30b02\u306f\u3001\u7d04100\u56de\u8ee2\u3067\u7834\u640d\u3057\u3001\u305d\u306e\u5f8c\u3001\u6469\u8017\u8a66\u9a13\u7d42\u4e86\u6642\u306bCOF\u304c\u7d040.5\u307e\u3067\u5927\u5e45\u306b\u5897\u52a0\u3057\u307e\u3057\u305f\u3002<\/span><\/p><p><span class=\"fontstyle0\"><br \/>\u30bb\u30eb\u30d5\u30af\u30ea\u30fc\u30f3\u30ac\u30e9\u30b9\u30b3\u30fc\u30c6\u30a3\u30f3\u30b0\u306e\u4f4e\u6469\u64e6\u306f\u3001\u8868\u9762\u30a8\u30cd\u30eb\u30ae\u30fc\u306e\u4f4e\u3055\u306b\u8d77\u56e0\u3057\u3066\u3044\u307e\u3059\u3002\u975e\u5e38\u306b\u9ad8\u3044\u9759\u96fb\u6c17\u3092\u767a\u751f\u3055\u305b\u308b<br \/>\u306e\u6c34\u63a5\u89e6\u89d2\u3068\u4f4e\u3044\u30ed\u30fc\u30eb\u30aa\u30d5\u89d2\u3092\u6301\u3064\u3002\u306e\u9855\u5fae\u93e1\u3067\u793a\u3059\u3088\u3046\u306b\u300190% RH\u306e\u30b3\u30fc\u30c6\u30a3\u30f3\u30b0\u8868\u9762\u306b\u5c0f\u3055\u306a\u6c34\u6ef4\u3092\u5f62\u6210\u3059\u308b\u3053\u3068\u306b\u306a\u308b\u3002 <\/span><span class=\"fontstyle2\">\u56f33<\/span><span class=\"fontstyle0\">.\u307e\u305f\u3001RH\u5024\u304c30%\u304b\u308990%\u306b\u4e0a\u6607\u3059\u308b\u3068\u3001Coating 2\u306e\u5e73\u5747COF\u306f\u301c0.23\u304b\u3089\u301c0.15\u306b\u6e1b\u5c11\u3057\u305f\u3002<\/span><\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<section class=\"elementor-section elementor-inner-section elementor-element elementor-element-eb4749e elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"eb4749e\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-inner-column elementor-element elementor-element-c5eb537\" data-id=\"c5eb537\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-02c5d46 elementor-widget elementor-widget-image\" data-id=\"02c5d46\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img loading=\"lazy\" decoding=\"async\" width=\"658\" height=\"523\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2021\/05\/Coefficient-of-friction-pin-on-disk-tests-in-different-relative-humidity.png\" class=\"attachment-large size-large wp-image-11421\" alt=\"\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-inner-column elementor-element elementor-element-204ed41\" data-id=\"204ed41\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-6fbd6ef elementor-widget elementor-widget-image\" data-id=\"6fbd6ef\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img loading=\"lazy\" decoding=\"async\" width=\"658\" height=\"523\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2021\/05\/COF-pin-on-disk-tests-in-different-relative-humidity.png\" class=\"attachment-large size-large wp-image-11420\" alt=\"\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-inner-section elementor-element elementor-element-9c7452f elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"9c7452f\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-33 elementor-inner-column elementor-element elementor-element-2a4b192\" data-id=\"2a4b192\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap\">\n\t\t\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t<div class=\"elementor-column elementor-col-33 elementor-inner-column elementor-element elementor-element-eec210a\" data-id=\"eec210a\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-13bab9f elementor-widget elementor-widget-image\" data-id=\"13bab9f\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img loading=\"lazy\" decoding=\"async\" width=\"658\" height=\"522\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2021\/05\/COF-during-the-pin-on-disk-tests-in-different-relative-humidity.png\" class=\"attachment-large size-large wp-image-11419\" alt=\"\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t<div class=\"elementor-column elementor-col-33 elementor-inner-column elementor-element elementor-element-6070530\" data-id=\"6070530\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap\">\n\t\t\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<div class=\"elementor-element elementor-element-e8744f2 elementor-widget elementor-widget-text-editor\" data-id=\"e8744f2\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p style=\"text-align: center;\"><span class=\"fontstyle0\" style=\"color: #1b96cf;\">\u56f31: <\/span><span class=\"fontstyle0\" style=\"color: #000000;\">\u76f8\u5bfe\u6e7f\u5ea6\u3092\u5909\u5316\u3055\u305b\u305f\u5834\u5408\u306e\u30d4\u30f3\u30aa\u30f3\u30c7\u30a3\u30b9\u30af\u8a66\u9a13\u6642\u306e\u6469\u64e6\u4fc2\u6570\u3002<\/span><\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-b8e9638 elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"b8e9638\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-efed3fb\" data-id=\"efed3fb\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<section class=\"elementor-section elementor-inner-section elementor-element elementor-element-a6f671e elementor-section-content-top elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"a6f671e\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-inner-column elementor-element elementor-element-d9e612f\" data-id=\"d9e612f\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-e5eb952 elementor-widget elementor-widget-image\" data-id=\"e5eb952\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img loading=\"lazy\" decoding=\"async\" width=\"699\" height=\"559\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2021\/05\/Average-COF-during-pin-on-disk-tests-in-different-relative-humidity.png\" class=\"attachment-large size-large wp-image-11400\" alt=\"\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-5aa1f26 elementor-widget elementor-widget-text-editor\" data-id=\"5aa1f26\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p style=\"text-align: center;\"><span class=\"fontstyle0\" style=\"color: #1b96cf;\">\u56f32: <\/span><span class=\"fontstyle0\" style=\"color: #000000;\">\u76f8\u5bfe\u6e7f\u5ea6\u3092\u5909\u5316\u3055\u305b\u305f\u5834\u5408\u306e\u30d4\u30f3\u30aa\u30f3\u30c7\u30a3\u30b9\u30af\u30c6\u30b9\u30c8\u306b\u304a\u3051\u308b\u5e73\u5747COF\u3002<\/span><\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-inner-column elementor-element elementor-element-df357c5\" data-id=\"df357c5\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-607f575 elementor-widget elementor-widget-image\" data-id=\"607f575\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img loading=\"lazy\" decoding=\"async\" width=\"671\" height=\"532\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2021\/05\/Formation-of-small-water-droplets-on-the-coated-glass-surface.png\" class=\"attachment-large size-large wp-image-11398\" alt=\"\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-9b68cea elementor-widget elementor-widget-text-editor\" data-id=\"9b68cea\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p style=\"text-align: center;\"><span class=\"fontstyle0\" style=\"color: #1b96cf;\">\u56f33: <\/span><span class=\"fontstyle0\" style=\"color: #000000;\">\u30b3\u30fc\u30c6\u30a3\u30f3\u30b0\u3055\u308c\u305f\u30ac\u30e9\u30b9\u8868\u9762\u306b\u5c0f\u3055\u306a\u6c34\u6ef4\u304c\u5f62\u6210\u3055\u308c\u308b\u3002<\/span><\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<div class=\"elementor-element elementor-element-4972b2b elementor-widget elementor-widget-text-editor\" data-id=\"4972b2b\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p><span class=\"fontstyle0\">\u56f34 <\/span><span class=\"fontstyle2\">\u306f\uff0c\u7570\u306a\u308b\u6e7f\u5ea6\u3067\u306e\u6469\u8017\u8a66\u9a13\u5f8c\u306e\u30ac\u30e9\u30b9\u8868\u9762\u306e\u6469\u8017\u75d5\u3092\u6bd4\u8f03\u3057\u305f\u3082\u306e\u3067\u3042\u308b\u3002\u30b3\u30fc\u30c6\u30a3\u30f3\u30b01\u306f\uff0c30%\u306860%\u306eRH\u3067\u6469\u8017\u8a66\u9a13\u3092\u884c\u3063\u305f\u5f8c\uff0c\u8efd\u5ea6\u306e\u6469\u8017\u306e\u5146\u5019\u3092\u793a\u3057\u3066\u3044\u308b\u300290%\u306eRH\u3067\u306f\u5927\u304d\u306a\u6469\u8017\u75d5\u304c\u898b\u3089\u308c\uff0c\u6469\u8017\u8a66\u9a13\u4e2d\u306eCOF\u306e\u5927\u5e45\u306a\u4e0a\u6607\u3068\u4e00\u81f4\u3057\u3066\u3044\u308b\u3002\u30b3\u30fc\u30c6\u30a3\u30f3\u30b02\u306f\uff0c\u4e7e\u6e7f\u4e21\u74b0\u5883\u3067\u306e\u6469\u8017\u8a66\u9a13\u3067\u307b\u3068\u3093\u3069\u6469\u8017\u304c\u898b\u3089\u308c\u305a\uff0c\u307e\u305f\uff0c\u7570\u306a\u308b\u6e7f\u5ea6\u3067\u306e\u6469\u8017\u8a66\u9a13\u3067\u4e00\u5b9a\u306e\u4f4e\u3044COF\u3092\u793a\u3057\u305f\u3002\u512a\u308c\u305f\u30c8\u30e9\u30a4\u30dc\u30ed\u30b8\u30fc\u7279\u6027\u3068\u4f4e\u3044\u8868\u9762\u30a8\u30cd\u30eb\u30ae\u30fc\u306e\u7d44\u307f\u5408\u308f\u305b\u306b\u3088\u308a\u3001Coating 2\u306f\u904e\u9177\u306a\u74b0\u5883\u4e0b\u3067\u306e\u30bb\u30eb\u30d5\u30af\u30ea\u30fc\u30cb\u30f3\u30b0\u30ac\u30e9\u30b9\u30b3\u30fc\u30c6\u30a3\u30f3\u30b0\u7528\u9014\u306b\u9069\u3057\u3066\u3044\u308b\u3053\u3068\u304c\u5206\u304b\u308a\u307e\u3059\u3002\u4e00\u65b9\u3001\u30b3\u30fc\u30c6\u30a3\u30f3\u30b0\u3055\u308c\u3066\u3044\u306a\u3044\u30ac\u30e9\u30b9\u306f\u3001\u7570\u306a\u308b\u6e7f\u5ea6\u74b0\u5883\u4e0b\u3067\u3088\u308a\u5927\u304d\u306a\u6469\u8017\u75d5\u3068\u3088\u308a\u9ad8\u3044COF\u3092\u793a\u3057\u3001\u30bb\u30eb\u30d5\u30af\u30ea\u30fc\u30cb\u30f3\u30b0\u30b3\u30fc\u30c6\u30a3\u30f3\u30b0\u6280\u8853\u306e\u5fc5\u8981\u6027\u3092\u793a\u3057\u3066\u3044\u308b\u3002<\/span><\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-ec86e16 elementor-widget elementor-widget-image\" data-id=\"ec86e16\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img loading=\"lazy\" decoding=\"async\" width=\"1024\" height=\"777\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2021\/05\/Wear-tracks-after-the-pin-on-disk-tests-in-different-relative-humidity-NANOVEA-Tribometer.png\" class=\"attachment-large size-large wp-image-11401\" alt=\"\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-41dd146 elementor-widget elementor-widget-text-editor\" data-id=\"41dd146\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p style=\"text-align: center;\"><span class=\"fontstyle0\" style=\"color: #1b96cf;\">\u56f34: <\/span><span class=\"fontstyle0\" style=\"color: #000000;\">\u76f8\u5bfe\u6e7f\u5ea6\u3092\u5909\u5316\u3055\u305b\u305f\u30d4\u30f3\u30aa\u30f3\u30c7\u30a3\u30b9\u30af\u8a66\u9a13\u5f8c\u306e\u6469\u8017\u75d5\uff08200\u500d\u62e1\u5927\uff09\u3002<\/span><\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-9c9a5b1 elementor-section-height-min-height elementor-section-content-middle elementor-reverse-mobile elementor-section-boxed elementor-section-height-default elementor-section-items-middle\" data-id=\"9c9a5b1\" data-element_type=\"section\" data-settings=\"{&quot;background_background&quot;:&quot;classic&quot;}\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-top-column elementor-element elementor-element-c893767\" data-id=\"c893767\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-6809f1b elementor-widget elementor-widget-image\" data-id=\"6809f1b\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img loading=\"lazy\" decoding=\"async\" width=\"419\" height=\"821\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2021\/05\/Glass-Coating-Humidity-Test-Conclusion.png\" class=\"attachment-large size-large wp-image-11407\" alt=\"\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-top-column elementor-element elementor-element-f2d1204\" data-id=\"f2d1204\" data-element_type=\"column\" data-settings=\"{&quot;background_background&quot;:&quot;classic&quot;}\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-784c0d2 elementor-widget elementor-widget-heading\" data-id=\"784c0d2\" data-element_type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\">\u307e\u3068\u3081<\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-445fc39 elementor-widget elementor-widget-text-editor\" data-id=\"445fc39\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p><span class=\"fontstyle2\"> <span class=\"fontstyle0\">\u30ca\u30ce\u30d3\u30a2 <\/span>T100\u30c8\u30e9\u30a4\u30dc\u30e1\u30fc\u30bf\u306f\u3001\u7570\u306a\u308b\u6e7f\u5ea6\u74b0\u5883\u4e0b\u3067\u306e\u30bb\u30eb\u30d5\u30af\u30ea\u30fc\u30cb\u30f3\u30b0\u30ac\u30e9\u30b9\u30b3\u30fc\u30c6\u30a3\u30f3\u30b0\u306e\u8a55\u4fa1\u3068\u54c1\u8cea\u7ba1\u7406\u306b\u6700\u9069\u306a\u30c4\u30fc\u30eb\u3067\u3059\u3002\u307e\u305f\u3001COF \u3092\u305d\u306e\u5834\u3067\u6e2c\u5b9a\u3067\u304d\u308b\u305f\u3081\u3001\u6469\u8017\u306e\u69d8\u3005\u306a\u6bb5\u968e\u3068 COF \u306e\u5909\u5316\u3092\u95a2\u9023\u4ed8\u3051\u308b\u3053\u3068\u304c\u3067\u304d\u3001\u30ac\u30e9\u30b9\u88ab\u819c\u306e\u6469\u8017\u30e1\u30ab\u30cb\u30ba\u30e0\u3084\u30c8\u30e9\u30a4\u30dc\u30ed\u30b8\u30fc\u7279\u6027\u306e\u57fa\u672c\u7684\u306a\u7406\u89e3\u3092\u6df1\u3081\u308b\u4e0a\u3067\u975e\u5e38\u306b\u91cd\u8981\u3067\u3042\u308b\u3002\u7570\u306a\u308b\u6e7f\u5ea6\u74b0\u5883\u3067\u8a66\u9a13\u3057\u305f\u30bb\u30eb\u30d5\u30af\u30ea\u30fc\u30cb\u30f3\u30b0\u30ac\u30e9\u30b9\u30b3\u30fc\u30c6\u30a3\u30f3\u30b0\u306e\u5305\u62ec\u7684\u306a\u30c8\u30e9\u30a4\u30dc\u30ed\u30b8\u30fc\u5206\u6790\u306b\u57fa\u3065\u304d\u3001\u30b3\u30fc\u30c6\u30a3\u30f3\u30b02\u306f\u4e7e\u71e5\u304a\u3088\u3073\u6e7f\u6f64\u74b0\u5883\u306e\u4e21\u65b9\u3067\u4e00\u5b9a\u306e\u4f4e\u3044COF\u3068\u512a\u308c\u305f\u8010\u6469\u8017\u6027\u3092\u6709\u3059\u308b\u3053\u3068\u3092\u793a\u3057\u3001\u7570\u306a\u308b\u5929\u5019\u306b\u3055\u3089\u3055\u308c\u308b\u30bb\u30eb\u30d5\u30af\u30ea\u30fc\u30cb\u30f3\u30b0\u30ac\u30e9\u30b9\u30b3\u30fc\u30c6\u30a3\u30f3\u30b0\u7528\u9014\u306b\u9069\u3057\u305f\u5019\u88dc\u3067\u3042\u308b\u3053\u3068\u304c\u5206\u304b\u3063\u305f\u3002<\/span><\/p><p><span class=\"fontstyle2\"><br \/><span class=\"fontstyle0\">\u30ca\u30ce\u30d3\u30a2 <\/span>\u30c8\u30e9\u30a4\u30dc\u30e1\u30fc\u30bf\u306f\u3001ISO\u3084ASTM\u306b\u6e96\u62e0\u3057\u305f\u56de\u8ee2\u30fb\u76f4\u52d5\u30e2\u30fc\u30c9\u306b\u3088\u308b\u7cbe\u5bc6\u3067\u518d\u73fe\u6027\u306e\u9ad8\u3044\u6469\u8017\u30fb\u6469\u64e6\u8a66\u9a13\u3068\u3001\u30aa\u30d7\u30b7\u30e7\u30f3\u3067\u9ad8\u6e29\u6469\u8017\u30fb\u6f64\u6ed1\u30fb\u30c8\u30e9\u30a4\u30dc\u30b3\u30ed\u30fc\u30b8\u30e7\u30f3\u30921\u3064\u306e\u30b7\u30b9\u30c6\u30e0\u306b\u7d71\u5408\u3057\u3066\u63d0\u4f9b\u3057\u307e\u3059\u3002\u30aa\u30d7\u30b7\u30e7\u30f3\u306e3D\u975e\u63a5\u89e6\u30d7\u30ed\u30d5\u30a1\u30a4\u30e9\u3092\u4f7f\u7528\u3059\u308c\u3070\u3001\u9ad8\u7cbe\u5ea6\u306a\u6469\u64e6\u8a66\u9a13\u3082\u53ef\u80fd\u3067\u3059\u3002<br \/>\u7c97\u3055\u306a\u3069\u306e\u4ed6\u306e\u8868\u9762\u6e2c\u5b9a\u306b\u52a0\u3048\u3066\u3001\u6469\u8017\u75d5\u306e\u5206\u89e3\u80fd\u306e\u9ad8\u30443D\u30a4\u30e1\u30fc\u30b8\u30f3\u30b0\u3092\u884c\u3044\u307e\u3059\u3002\u00a0<\/span><\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-ed1114a elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"ed1114a\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-bf4d8c6\" data-id=\"bf4d8c6\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-56694c0 elementor-widget elementor-widget-heading\" data-id=\"56694c0\" data-element_type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\">\u540c\u3058\u3088\u3046\u306a\u30a2\u30d7\u30ea\u30b1\u30fc\u30b7\u30e7\u30f3\u3092\u304a\u6301\u3061\u3067\u3059\u304b\uff1f<\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-62d26b1 elementor-align-justify open-chat elementor-widget elementor-widget-button\" data-id=\"62d26b1\" data-element_type=\"widget\" data-widget_type=\"button.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<div class=\"elementor-button-wrapper\">\n\t\t\t\t\t<a class=\"elementor-button elementor-size-sm\" role=\"button\">\n\t\t\t\t\t\t<span class=\"elementor-button-content-wrapper\">\n\t\t\t\t\t\t\t\t\t<span class=\"elementor-button-text\">\u5c02\u9580\u5bb6\u306b\u76f8\u8ac7\u3059\u308b<\/span>\n\t\t\t\t\t<\/span>\n\t\t\t\t\t<\/a>\n\t\t\t\t<\/div>\n\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-651044a elementor-align-justify button-quote elementor-widget elementor-widget-button\" data-id=\"651044a\" data-element_type=\"widget\" data-widget_type=\"button.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<div class=\"elementor-button-wrapper\">\n\t\t\t\t\t<a class=\"elementor-button elementor-button-link elementor-size-sm\" href=\"https:\/\/nanovea.com\/contact-sales-form\/\" id=\"button-quote-bottom\">\n\t\t\t\t\t\t<span class=\"elementor-button-content-wrapper\">\n\t\t\t\t\t\t\t\t\t<span class=\"elementor-button-text\">\u4fa1\u683c\u3068\u8a73\u7d30\u3092\u7d20\u65e9\u304f\u5165\u624b<\/span>\n\t\t\t\t\t<\/span>\n\t\t\t\t\t<\/a>\n\t\t\t\t<\/div>\n\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<\/div>","protected":false},"excerpt":{"rendered":"<p>\u30c8\u30e9\u30a4\u30dc\u30e1\u30fc\u30bf\u306b\u3088\u308b\u30ac\u30e9\u30b9\u30b3\u30fc\u30c6\u30a3\u30f3\u30b0\u306e\u6e7f\u5ea6\u6469\u8017\u8a66\u9a13 \u8a73\u7d30\u306f\u3053\u3061\u3089<\/p>","protected":false},"author":1,"featured_media":16869,"comment_status":"open","ping_status":"open","sticky":false,"template":"","format":"standard","meta":{"_exactmetrics_skip_tracking":false,"_exactmetrics_sitenote_active":false,"_exactmetrics_sitenote_note":"","_exactmetrics_sitenote_category":0,"footnotes":""},"categories":[7,382,349,373,336],"tags":[],"class_list":["post-11395","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-application-notes","category-humidity-gases-tribology","category-laboratory-testing","category-rotational-tribology","category-tribology-testing"],"_links":{"self":[{"href":"https:\/\/nanovea.com\/ja\/wp-json\/wp\/v2\/posts\/11395","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/nanovea.com\/ja\/wp-json\/wp\/v2\/posts"}],"about":[{"href":"https:\/\/nanovea.com\/ja\/wp-json\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"https:\/\/nanovea.com\/ja\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/nanovea.com\/ja\/wp-json\/wp\/v2\/comments?post=11395"}],"version-history":[{"count":46,"href":"https:\/\/nanovea.com\/ja\/wp-json\/wp\/v2\/posts\/11395\/revisions"}],"predecessor-version":[{"id":24743,"href":"https:\/\/nanovea.com\/ja\/wp-json\/wp\/v2\/posts\/11395\/revisions\/24743"}],"wp:featuredmedia":[{"embeddable":true,"href":"https:\/\/nanovea.com\/ja\/wp-json\/wp\/v2\/media\/16869"}],"wp:attachment":[{"href":"https:\/\/nanovea.com\/ja\/wp-json\/wp\/v2\/media?parent=11395"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"https:\/\/nanovea.com\/ja\/wp-json\/wp\/v2\/categories?post=11395"},{"taxonomy":"post_tag","embeddable":true,"href":"https:\/\/nanovea.com\/ja\/wp-json\/wp\/v2\/tags?post=11395"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}