{"id":214,"date":"2015-03-04T17:48:59","date_gmt":"2015-03-04T17:48:59","guid":{"rendered":"http:\/\/nanovea.com\/?page_id=214"},"modified":"2019-11-13T16:47:46","modified_gmt":"2019-11-13T16:47:46","slug":"%e5%9b%9e%e8%bb%a2%e6%b6%88%e8%80%97%e8%a9%a6%e9%a8%93","status":"publish","type":"page","link":"https:\/\/nanovea.com\/ja\/rotative-wear-test\/","title":{"rendered":"\u56de\u8ee2\u6469\u8017\u8a66\u9a13"},"content":{"rendered":"<div class=\"wonderpluginslider-container\" id=\"wonderpluginslider-container-17\" style=\"max-width:1035px;margin:0 auto;padding-left:0px;padding-right:0px;padding-top:0px;padding-bottom:0px;\"><div class=\"wonderpluginslider\" id=\"wonderpluginslider-17\" data-sliderid=\"17\" data-width=\"1035\" data-height=\"375\" data-skin=\"cube\" data-autoplay=\"true\" data-randomplay=\"false\" data-loadimageondemand=\"false\" data-transitiononfirstslide=\"false\" data-autoplayvideo=\"false\" data-isresponsive=\"true\" data-fullwidth=\"false\" data-isfullscreen=\"false\" data-ratioresponsive=\"false\" data-showtext=\"true\" data-showtimer=\"false\" data-showbottomshadow=\"false\" data-navshowpreview=\"false\" data-textautohide=\"true\" data-pauseonmouseover=\"false\" data-lightboxresponsive=\"true\" data-lightboxshownavigation=\"false\" data-lightboxshowtitle=\"true\" data-lightboxshowdescription=\"false\" data-texteffectresponsive=\"true\" data-donotinit=\"false\" data-addinitscript=\"false\" data-lightboxfullscreenmode=\"false\" data-lightboxcloseonoverlay=\"true\" data-lightboxvideohidecontrols=\"false\" data-lightboxnogroup=\"false\" data-shownav=\"true\" data-navthumbresponsive=\"false\" data-navshowfeaturedarrow=\"false\" data-lightboxshowsocial=\"false\" data-lightboxshowfacebook=\"true\" data-lightboxshowtwitter=\"true\" data-lightboxshowpinterest=\"true\" data-lightboxsocialrotateeffect=\"true\" data-showsocial=\"false\" data-showfacebook=\"true\" data-showtwitter=\"true\" data-showpinterest=\"true\" data-socialrotateeffect=\"true\" data-disableinlinecss=\"false\" data-triggerresize=\"false\" data-lightboxautoslide=\"false\" data-lightboxshowtimer=\"true\" data-lightboxshowplaybutton=\"true\" data-lightboxalwaysshownavarrows=\"false\" data-lightboxshowtitleprefix=\"true\" data-titleusealt=\"false\" data-outputtext=\"false\" data-scalemode=\"fit\" data-arrowstyle=\"always\" data-transition=\"slide\" data-loop=\"0\" data-border=\"0\" data-slideinterval=\"8000\" data-arrowimage=\"arrows-36-80-0.png\" data-arrowwidth=\"36\" data-arrowheight=\"80\" data-arrowtop=\"50\" data-arrowmargin=\"-18\" data-navstyle=\"bullets\" data-navimage=\"bullet-24-24-1.png\" data-navwidth=\"24\" data-navheight=\"24\" data-navspacing=\"8\" data-navmarginx=\"16\" data-navmarginy=\"16\" data-navposition=\"bottom\" data-navthumbnavigationstyle=\"arrow\" data-navthumbnavigationarrowimage=\"carouselarrows-32-32-0.png\" data-navthumbnavigationarrowimagewidth=\"32\" data-navthumbnavigationarrowimageheight=\"32\" data-playvideoimage=\"playvideo-64-64-0.png\" data-playvideoimagewidth=\"64\" data-playvideoimageheight=\"64\" data-lightboxthumbwidth=\"90\" data-lightboxthumbheight=\"60\" data-lightboxthumbtopmargin=\"12\" data-lightboxthumbbottommargin=\"4\" data-lightboxbarheight=\"64\" data-lightboxtitlebottomcss=\"color:#333; font-size:14px; font-family:Armata,sans-serif,Arial; overflow:hidden; text-align:left;\" data-lightboxdescriptionbottomcss=\"color:#333; font-size:12px; font-family:Arial,Helvetica,sans-serif; overflow:hidden; text-align:left; margin:4px 0px 0px; padding: 0px;\" data-textformat=\"Color box\" data-textpositionstatic=\"bottom\" data-textpositiondynamic=\"topleft\" data-paddingleft=\"0\" data-paddingright=\"0\" data-paddingtop=\"0\" data-paddingbottom=\"0\" data-texteffectresponsivesize=\"640\" data-textleftrightpercentforstatic=\"40\" data-fadeduration=\"1000\" data-crossfadeduration=\"1000\" data-fadeoutfadeinduration=\"2000\" data-slideduration=\"1000\" data-elasticduration=\"1000\" data-sliceduration=\"1500\" data-blindsduration=\"1500\" data-blocksduration=\"1500\" data-shuffleduration=\"1500\" data-tilesduration=\"2000\" data-kenburnsduration=\"5000\" data-flipduration=\"1500\" data-flipwithzoomduration=\"2000\" data-threedduration=\"1500\" data-threedhorizontalduration=\"1500\" data-threedwithzoomduration=\"2500\" data-threedhorizontalwithzoomduration=\"2200\" data-threedflipduration=\"1500\" data-threedflipwithzoomduration=\"2000\" data-threedtilesduration=\"2000\" data-threedfallback=\"flip\" data-threedhorizontalfallback=\"flip\" data-threedwithzoomfallback=\"flipwithzoom\" data-threedhorizontalwithzoomfallback=\"flipwithzoom\" data-threedflipfallback=\"flip\" data-threedflipwithzoomfallback=\"flipwithzoom\" data-threedtilesfallback=\"tiles\" data-ratiomediumscreen=\"800\" data-ratiomediumheight=\"1.2\" data-ratiosmallscreen=\"480\" data-ratiosmallheight=\"1.6\" data-socialmode=\"mouseover\" data-socialposition=\"position:absolute;top:8px;right:8px;\" data-socialpositionsmallscreen=\"position:absolute;top:8px;right:8px;\" data-socialdirection=\"horizontal\" data-socialbuttonsize=\"32\" data-socialbuttonfontsize=\"18\" data-navthumbcolumn=\"5\" data-navthumbtitleheight=\"20\" data-navthumbtitlewidth=\"120\" data-navthumbresponsivemode=\"samesize\" data-navthumbstyle=\"imageonly\" data-navthumbmediumsize=\"900\" data-navthumbmediumwidth=\"64\" data-navthumbmediumheight=\"64\" data-navthumbmediumcolumn=\"4\" data-navthumbmediumtitleheight=\"18\" data-navthumbmediumtitlewidth=\"120\" data-navthumbsmallsize=\"600\" data-navthumbsmallwidth=\"48\" data-navthumbsmallheight=\"48\" data-navthumbsmallcolumn=\"3\" data-navthumbsmalltitleheight=\"18\" data-navthumbsmalltitlewidth=\"120\" data-lightboxsocialposition=\"position:absolute;top:100%;right:0;\" data-lightboxsocialpositionsmallscreen=\"position:absolute;top:100%;right:0;left:0;\" data-lightboxsocialdirection=\"horizontal\" data-lightboxsocialbuttonsize=\"32\" data-lightboxsocialbuttonfontsize=\"18\" data-lightboxtitlestyle=\"bottom\" data-lightboximagepercentage=\"75\" data-lightboxdefaultvideovolume=\"1\" data-lightboxoverlaybgcolor=\"#000\" data-lightboxoverlayopacity=\"0.9\" data-lightboxbgcolor=\"#fff\" data-lightboxtitleprefix=\"%NUM \/ %TOTAL\" data-lightboxtitleinsidecss=\"color:#fff; font-size:16px; font-family:Arial,Helvetica,sans-serif; overflow:hidden; text-align:left;\" data-lightboxdescriptioninsidecss=\"color:#fff; font-size:12px; font-family:Arial,Helvetica,sans-serif; overflow:hidden; text-align:left; margin:4px 0px 0px; padding: 0px;\" data-triggerresizedelay=\"100\" data-lightboxslideinterval=\"5000\" data-lightboxtimerposition=\"bottom\" data-lightboxtimercolor=\"#dc572e\" data-lightboxtimeropacity=\"1\" data-lightboxbordersize=\"8\" data-lightboxborderradius=\"0\" data-textcss=\"display:block; padding:8px 16px; text-align:left;\" data-textbgcss=\"display:none;\" data-titlecss=\"color: #1b96cf;    font-family: &quot;Open Sans&quot;,sans-serif;    font-size: 32px;    font-weight: bold;    line-height: 44px;    margin-bottom: 0;    margin-top: 20px;    text-transform: uppercase;\" data-descriptioncss=\"color: #282828;    font-size: 18px;    line-height: 30px;\" data-buttoncss=\"display:block; position:relative; margin-top:10px;\" data-titlecssresponsive=\"font-size:12px;\" data-descriptioncssresponsive=\"display:none !important;\" data-buttoncssresponsive=\"font-size: 9px !important;width:100%;\" data-jsfolder=\"https:\/\/nanovea.com\/wp-content\/plugins\/wonderplugin-slider-lite\/engine\/\" style=\"display:none;\" ><ul class=\"amazingslider-slides\"  style=\"display:none;\"><li><img decoding=\"async\" class=\"amazingslider-img-elem amazingsliderimg\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2018\/01\/slide-rotative-wear-test.jpg\" alt=\"\u56de\u8ee2\u78e8\u8017\u6469\u64e6\" title=\"\u56de\u8ee2\u78e8\u8017\u6469\u64e6\" data-description=\"Precise and flexable testing with &lt;br \/&gt;unmatched speed controls\" \/><\/li><li><img decoding=\"async\" class=\"amazingslider-img-elem amazingsliderimg\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2015\/04\/rotative-wear-friction-depth.jpg\" alt=\"\u56de\u8ee2\u78e8\u8017\u6469\u64e6\" title=\"\u56de\u8ee2\u78e8\u8017\u6469\u64e6\" data-description=\"Continuous coefficient of friction &amp; depth by &lt;br \/&gt;LVDT or depth by in-situ optical profiler\" \/><\/li><li><img decoding=\"async\" class=\"amazingslider-img-elem amazingsliderimg\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2015\/04\/rotative-wear-friction-speed.jpg\" alt=\"\u56de\u8ee2\u78e8\u8017\u6469\u64e6\" title=\"\u56de\u8ee2\u78e8\u8017\u6469\u64e6\" data-description=\"Unmatched speed control: wear rate vs. time, &lt;br \/&gt;quasi static friction &amp; continuous stribeck curves\" \/><\/li><\/ul><\/div><\/div><div id=\"amazingslider_customtexteffect_17\" style=\"display:none;\" data-texteffect=\"{&quot;Color box&quot;:{&quot;textstyle&quot;:&quot;dynamic&quot;,&quot;textpositionstatic&quot;:&quot;bottom&quot;,&quot;textautohide&quot;:true,&quot;textpositionmarginstatic&quot;:0,&quot;textpositiondynamic&quot;:&quot;topleft&quot;,&quot;textpositionmarginleft&quot;:24,&quot;textpositionmarginright&quot;:24,&quot;textpositionmargintop&quot;:24,&quot;textpositionmarginbottom&quot;:24,&quot;texteffect&quot;:&quot;slide&quot;,&quot;texteffecteasing&quot;:&quot;easeOutCubic&quot;,&quot;texteffectduration&quot;:600,&quot;texteffectslidedirection&quot;:&quot;left&quot;,&quot;texteffectslidedistance&quot;:30,&quot;texteffectdelay&quot;:500,&quot;texteffectseparate&quot;:true,&quot;texteffect1&quot;:&quot;slide&quot;,&quot;texteffectslidedirection1&quot;:&quot;right&quot;,&quot;texteffectslidedistance1&quot;:120,&quot;texteffecteasing1&quot;:&quot;easeOutCubic&quot;,&quot;texteffectduration1&quot;:600,&quot;texteffectdelay1&quot;:1000,&quot;texteffect2&quot;:&quot;slide&quot;,&quot;texteffectslidedirection2&quot;:&quot;right&quot;,&quot;texteffectslidedistance2&quot;:120,&quot;texteffecteasing2&quot;:&quot;easeOutCubic&quot;,&quot;texteffectduration2&quot;:600,&quot;texteffectdelay2&quot;:1500,&quot;textcss&quot;:&quot;display:block; padding:8px 16px; text-align:left;&quot;,&quot;textbgcss&quot;:&quot;display:none;&quot;,&quot;titlecss&quot;:&quot;color: #1b96cf;\\n    font-family: \\&quot;Open Sans\\&quot;,sans-serif;\\n    font-size: 32px;\\n    font-weight: bold;\\n    line-height: 44px;\\n    margin-bottom: 0;\\n    margin-top: 20px;\\n    text-transform: uppercase;&quot;,&quot;descriptioncss&quot;:&quot;color: #282828;\\n    font-size: 18px;\\n    line-height: 30px;&quot;,&quot;buttoncss&quot;:&quot;display:block; position:relative; margin-top:10px;&quot;,&quot;texteffectresponsive&quot;:true,&quot;texteffectresponsivesize&quot;:640,&quot;titlecssresponsive&quot;:&quot;font-size:12px;&quot;,&quot;descriptioncssresponsive&quot;:&quot;display:none !important;&quot;,&quot;buttoncssresponsive&quot;:&quot;font-size: 9px !important;\\nwidth:100%;&quot;,&quot;addgooglefonts&quot;:false,&quot;googlefonts&quot;:&quot;&quot;,&quot;textleftrightpercentforstatic&quot;:40}}\"><\/div>\n<h1><strong>\u56de\u8ee2\u78e8\u8017\u6469\u64e6\u30a4\u30f3\u30c8\u30ed<\/strong><\/h1>\n<p><a href=\"https:\/\/nanovea.com\/tribometers\">\u30c8\u30e9\u30a4\u30dc\u30e1\u30fc\u30bf\u6a5f\u5668<\/a> | <a href=\"https:\/\/nanovea.com\/lab-services\/\">\u30e9\u30dc\u30b5\u30fc\u30d3\u30b9<\/a> | <a href=\"https:\/\/nanovea.com\/linear-wear-test\">\u30ea\u30cb\u30a2<\/a> | <a href=\"https:\/\/nanovea.com\/application-notes\">\u30a2\u30d7\u30ea\u30b1\u30fc\u30b7\u30e7\u30f3\u30ce\u30fc\u30c8<\/a><\/p>\n<div class=\"product-desc\">\n<p align=\"justify\"><strong>\u56de\u8ee2\u78e8\u8017\u306e\u6469\u64e6\u904e\u7a0b\u3002<\/strong><br \/>\n\u56de\u8ee2\u6469\u8017\u6469\u64e6\u8a66\u9a13\u306f\u3001\u73fe\u5b9f\u306e\u591a\u304f\u306e\u30c8\u30e9\u30a4\u30dc\u30ed\u30b8\u30fc\u6a5f\u69cb\u306b\u898b\u3089\u308c\u308b\u56de\u8ee2\u904b\u52d5\u3092\u518d\u73fe\u3057\u307e\u3059\u3002\u30d5\u30e9\u30c3\u30c8\u30c1\u30c3\u30d7\u3001\u30d4\u30f3\u30c1\u30c3\u30d7\u3001\u30dc\u30fc\u30eb\u30c1\u30c3\u30d7\u306e\u3044\u305a\u308c\u304b\u3092\u3001\u56de\u8ee2\u4e2d\u5fc3\u304b\u3089\u7279\u5b9a\u306e\u4f4d\u7f6e\u3067\u3001\u6b63\u78ba\u306a\u91cd\u3055\u3067\u8a66\u9a13\u30b5\u30f3\u30d7\u30eb\u306b\u88c5\u7740\u3057\u307e\u3059\u3002\u8a66\u6599\u304c\u56de\u8ee2\u3057\u59cb\u3081\u308b\u3068\u3001\u30c1\u30c3\u30d7\u306f\u56de\u8ee2\u6469\u8017\u75d5\u3092\u5f62\u6210\u3057\u307e\u3059\u3002\u6469\u64e6\u4fc2\u6570\u306f\u3001\u7cbe\u5bc6\u306b\u6821\u6b63\u3055\u308c\u305f\u30ed\u30fc\u30c9\u30bb\u30eb\u306e\u305f\u308f\u307f\u91cf\u306b\u3088\u3063\u3066\u6b63\u78ba\u306b\u6e2c\u5b9a\u3055\u308c\u307e\u3059\u300216bit\u306e\u5916\u90e8\u4f4d\u7f6e\u30a8\u30f3\u30b3\u30fc\u30c0\u3092\u5185\u8535\u3057\u3066\u3044\u308b\u305f\u3081\u3001\u5404\u30b5\u30a4\u30af\u30eb\u30d1\u30b9\u306b\u304a\u3051\u308b\u7279\u5b9a\u306e\u4f4d\u7f6e\u3084\u30be\u30fc\u30f3\u3067\u306e\u6469\u64e6\u3092\u8868\u793a\u3059\u308b\u3053\u3068\u304c\u3067\u304d\u307e\u3059\u3002\u307e\u305f\u300120\u30d3\u30c3\u30c8\u306e\u30b9\u30d4\u30fc\u30c9\u30a8\u30f3\u30b3\u30fc\u30c0\u3092\u5185\u8535\u3057\u3066\u3044\u308b\u305f\u3081\u30011\u56de\u306e\u8a66\u9a13\u30670.01\uff5e5000rpm\u306e\u56de\u8ee2\u901f\u5ea6\u3092\u30b9\u30e0\u30fc\u30ba\u306b\u5909\u5316\u3055\u305b\u3001\u6b63\u78ba\u306a\u6469\u64e6\u4fc2\u6570\u3092\u5f97\u308b\u3053\u3068\u304c\u3067\u304d\u307e\u3059\u30020.01rpm\u307e\u3067\u306e\u56de\u8ee2\u6570\u306f\u3001\u9759\u6b62\u57df\u3067\u306e\u6469\u64e6\u3092\u8abf\u3079\u305f\u308a\u3001\u9759\u6469\u64e6\u4fc2\u6570\u3068\u52d5\u6469\u64e6\u4fc2\u6570\u306e\u9593\u306e\u63a8\u79fb\u3092\u3088\u308a\u826f\u304f\u7406\u89e3\u3059\u308b\u305f\u3081\u306b\u4e0d\u53ef\u6b20\u3067\u3059\u3002  \u8a66\u6599\u306e\u6469\u8017\u901f\u5ea6\u306f\u3001\u9078\u629e\u3057\u305f\u4f4d\u7f6e\u306e2\u6b21\u5143\u30d7\u30ed\u30d5\u30a1\u30a4\u30eb\u3001\u307e\u305f\u306f\u6469\u8017\u75d5\u5168\u4f53\u306e\u5b9f\u969b\u306e3\u6b21\u5143\u30d7\u30ed\u30d5\u30a1\u30a4\u30eb\u304b\u3089\u8a08\u7b97\u3067\u304d\u307e\u3059\u3002\u30b9\u30d1\u30a4\u30e9\u30eb\u8a66\u9a13\u306f\u3001\u5168\u9577\u306b\u308f\u305f\u3063\u3066\u6bd4\u8f03\u53ef\u80fd\u306a\u6469\u64e6\u30c7\u30fc\u30bf\u3092\u5f97\u308b\u305f\u3081\u306b\u3001\u4efb\u610f\u306e\u4f4d\u7f6e\u3067\u4e00\u5b9a\u306e\u7dda\u901f\u5ea6\uff08\u56de\u8ee2\u901f\u5ea6\u3092\u5909\u66f4\uff09\u3067\u5b9f\u65bd\u3059\u308b\u3053\u3068\u304c\u3067\u304d\u307e\u3059\u3002<\/p>\n<p>&nbsp;<\/p>\n<p><strong>\u898f\u683c\u3067\u3059\u3002<\/strong><\/p>\n<p>- ASTM G99<\/p>\n<p>- DIN 50324<\/p>\n<p>- ASTM D3702<\/p>\n<p>- ASTM D2266<\/p>\n<p>- ASTM D4172<\/p>\n<p>- ASTM G132<\/p>\n<p>&nbsp;<\/p>\n<p><strong>\u56de\u8ee2\u78e8\u8017\u6469\u64e6\u8a66\u9a13\u3067\u89e3\u6790\u3057\u305f\u7279\u6027\u3002<\/strong><\/p>\n<p>- \u6469\u64e6\u4fc2\u6570<\/p>\n<p>- \u88c5\u7740\u7387<\/p>\n<p>- \u6545\u969c\u306e\u30dd\u30a4\u30f3\u30c8<\/p>\n<p>- \u96fb\u6c17\u62b5\u6297<\/p>\n<p>- \u6f64\u6ed1\u30fb\u8150\u98df\u7814\u7a76<\/p>\n<p>- \u6469\u64e6\u3068\u901f\u5ea6\u306e\u95a2\u4fc2<\/p>\n<p>- \u30b9\u30c8\u30ea\u30d9\u30c3\u30af\u30ab\u30fc\u30d6<\/p>\n<p>- \u30b9\u30af\u30e9\u30c3\u30c1\u30cf\u30fc\u30c9\u30cd\u30b9<\/p>\n<p>- \u9759\u6469\u64e6\u4fc2\u6570\u3001\u4ed6\u591a\u6570<\/p>\n<p>&nbsp;<\/p>\n<p><strong>\u56de\u8ee2\u6469\u8017\u6469\u64e6\u8a66\u9a13\u30bd\u30d5\u30c8\u30a6\u30a7\u30a2\u306e\u7279\u5fb4\u3002<\/strong><\/p>\n<p>- \u9023\u7d9a\u30b9\u30c8\u30ea\u30d9\u30c3\u30af\u30ab\u30fc\u30d6<\/p>\n<p>- \u751f\u30c7\u30fc\u30bf\u3068\u753b\u50cf\u306e\u66f8\u304d\u51fa\u3057<\/p>\n<p>- \u30ea\u30a2\u30eb\u30bf\u30a4\u30e0\u8868\u793a<\/p>\n<p>- \u81ea\u52d5\u30ec\u30dd\u30fc\u30c6\u30a3\u30f3\u30b0<\/p>\n<p>- \u591a\u8a00\u8a9e\u5bfe\u5fdc<\/p>\n<p>- \u30b9\u30af\u30e9\u30c3\u30c1\u786c\u5ea6\u8a08\u7b97<\/p>\n<p>- \u30b9\u30d4\u30fc\u30c9\u306b\u5909\u5316\u3092\u6301\u305f\u305b\u305f\u30de\u30af\u30ed<\/p>\n<p>- \u7dda\u901f\u5ea6\u4e00\u5b9a\u3067\u306e\u30b9\u30d1\u30a4\u30e9\u30eb\u30c6\u30b9\u30c8<\/p>\n<p>- \u56fa\u5b9a\u30b5\u30a4\u30af\u30eb\u8868\u793a<\/p>\n<p>- 360\u00b0\u30b5\u30a4\u30af\u30eb\u30b3\u30f3\u30da\u30a2\u30d3\u30e5\u30fc<\/p>\n<p>- \u81ea\u52d5\u6469\u8017\u8a08\u7b97<\/p>\n<p>- \u30bb\u30df\u30ea\u30cb\u30a2\uff08\u30df\u30af\u30ed\u30f3\u307e\u305f\u306f\u7a0b\u5ea6\uff09<\/p>\n<p>- \u30c6\u30b9\u30c8\u6642\u306e\u53ef\u5909\u901f\u5236\u5fa1\u3001\u4ed6\u591a\u6570<\/p>\n<p>&nbsp;<\/p>\n<p><strong>\u30c1\u30c3\u30d7(\u30c0\u30a4\u30e4\u30e2\u30f3\u30c9\u3001WC\u3001\u30b4\u30e0\u3001\u305d\u306e\u4ed6\u591a\u304f\u306e\u6750\u6599\uff09\u3002<\/strong><\/p>\n<p>- 3\u30016\u300110\u300125mm\u30dc\u30fc\u30eb<\/p>\n<p>- \u30ab\u30b9\u30bf\u30e0\u30dc\u30fc\u30eb\u30b5\u30a4\u30ba<\/p>\n<p>- \u30ab\u30b9\u30bf\u30e0\u30d4\u30f3\u30ba<\/p>\n<p>- \u30d5\u30e9\u30c3\u30c8\u30d7\u30ec\u30fc\u30c8<\/p>\n<p>- \u30ab\u30b9\u30bf\u30e0\u30b8\u30aa\u30e1\u30c8\u30ea\u30fc<\/p>\n<p>&nbsp;<\/p>\n<p><strong>\u74b0\u5883\u6761\u4ef6\u3002<\/strong><\/p>\n<p>- 1200\u2103\u30d5\u30eb\u30ea\u30e0\u30fc\u30d0\u30d6\u30eb\u30aa\u30fc\u30d6\u30f3<\/p>\n<p>- 150\u2103\u307e\u3067\u306e\u51b7\u5374<\/p>\n<p>- \u6db2\u4f53\u30ab\u30c3\u30d7\uff06\u6db2\u4f53\u52a0\u71b1\uff08150\u2103\u307e\u3067<\/p>\n<p>- \u6f64\u6ed1\u5264 Drop by Drop<\/p>\n<p>- \u6e7f\u5ea6\u30b3\u30f3\u30c8\u30ed\u30fc\u30eb<\/p>\n<p>- \u5404\u7a2e\u30ac\u30b9<\/p>\n<p>- \u771f\u7a7a<\/p>\n<p>&nbsp;<\/p>\n<p><strong>\u30b5\u30f3\u30d7\u30eb(s)\u30db\u30eb\u30c0\u30fc\u3002<\/strong><\/p>\n<p>- \u6a19\u6e96\u30af\u30e9\u30f3\u30d7<\/p>\n<p>- \u30d9\u30fc\u30b9\u30d7\u30ec\u30fc\u30c8\u3078\u306e\u30af\u30ea\u30c3\u30d7\u53d6\u308a\u4ed8\u3051<\/p>\n<p>- \u591a\u69d8\u306a\u5f62\u72b6\u306b\u5bfe\u5fdc\u3059\u308b\u30ab\u30b9\u30bf\u30e0\u30db\u30eb\u30c0\u30fc<\/p>\n<p>&nbsp;<\/p>\n<p><strong>\u56de\u8ee2\u5f0f\u8a66\u9a13\u30e2\u30fc\u30c9\u3002<\/strong><\/p>\n<p><a href=\"https:\/\/nanovea.com\/temperature-tribology-testing\" target=\"_blank\" rel=\"noopener noreferrer\">\u6e29\u5ea6\u30c8\u30e9\u30a4\u30dc\u30ed\u30b8\u30fc\u8a66\u9a13<\/a><\/p>\n<p><a href=\"https:\/\/nanovea.com\/liquid-tribology-testing\" target=\"_blank\" rel=\"noopener noreferrer\">\u6db2\u4e2d\u30c8\u30e9\u30a4\u30dc\u30ed\u30b8\u30fc\u8a66\u9a13 <\/a><\/p>\n<\/div>","protected":false},"excerpt":{"rendered":"<p>ROTATIONAL WEAR FRICTION INTRO Tribometer Instruments | Lab Services | Linear | Application Notes Rotational Wear Friction Process: Rotational wear friction test reproduces the rotational motion found in many real-world tribology mechanisms. A flat, pin or ball tip is loaded onto a test sample with a precise weight and at a specific position from the center of rotation. As the sample starts rotating, the tip creates a rotational wear track. Friction coefficient is accurately measured by the deflection of a load cell, precisely calibrated. Because of the integrated 16bit external position encoder, friction can be displayed for any specific position or zone for each cycle pass. Additionally, the internal 20bit [&hellip;]<\/p>\n","protected":false},"author":1,"featured_media":0,"parent":0,"menu_order":0,"comment_status":"open","ping_status":"open","template":"tpl-newslider.php","meta":{"_exactmetrics_skip_tracking":false,"_exactmetrics_sitenote_active":false,"_exactmetrics_sitenote_note":"","_exactmetrics_sitenote_category":0,"footnotes":""},"class_list":["post-214","page","type-page","status-publish","hentry"],"_links":{"self":[{"href":"https:\/\/nanovea.com\/ja\/wp-json\/wp\/v2\/pages\/214","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/nanovea.com\/ja\/wp-json\/wp\/v2\/pages"}],"about":[{"href":"https:\/\/nanovea.com\/ja\/wp-json\/wp\/v2\/types\/page"}],"author":[{"embeddable":true,"href":"https:\/\/nanovea.com\/ja\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/nanovea.com\/ja\/wp-json\/wp\/v2\/comments?post=214"}],"version-history":[{"count":22,"href":"https:\/\/nanovea.com\/ja\/wp-json\/wp\/v2\/pages\/214\/revisions"}],"predecessor-version":[{"id":7470,"href":"https:\/\/nanovea.com\/ja\/wp-json\/wp\/v2\/pages\/214\/revisions\/7470"}],"wp:attachment":[{"href":"https:\/\/nanovea.com\/ja\/wp-json\/wp\/v2\/media?parent=214"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}