{"id":8403,"date":"2019-05-12T13:32:24","date_gmt":"2019-05-12T13:32:24","guid":{"rendered":"https:\/\/nanovea.com\/?p=8403"},"modified":"2023-11-13T22:38:12","modified_gmt":"2023-11-13T22:38:12","slug":"test-di-usura-del-legno-con-il-tribometro-di-nanovea","status":"publish","type":"post","link":"https:\/\/nanovea.com\/it\/test-di-usura-del-legno-con-il-tribometro-di-nanovea\/","title":{"rendered":"Test di usura del legno con il tribometro Nanovea"},"content":{"rendered":"<div data-elementor-type=\"wp-post\" data-elementor-id=\"8403\" class=\"elementor elementor-8403\" data-elementor-post-type=\"post\">\n\t\t\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-3127429d elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"3127429d\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-4aead9d\" data-id=\"4aead9d\" data-element_type=\"column\" data-settings=\"{&quot;background_background&quot;:&quot;classic&quot;}\">\n\t\t\t<div class=\"elementor-widget-wrap\">\n\t\t\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-482f6253 elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"482f6253\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-270b5199\" data-id=\"270b5199\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-3131792c elementor-widget elementor-widget-text-editor\" data-id=\"3131792c\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p style=\"text-align: left; color: #1b96cf; font-size: 24px;\">Importanza del confronto tra usura e COF della finitura del legno<strong><u><i><br><\/i><\/u><\/strong><\/p>\n<p>Il legno \u00e8 stato utilizzato per migliaia di anni come materiale da costruzione per case, mobili e pavimenti. Ha una combinazione di bellezza naturale e durabilit\u00e0, che lo rendono un candidato ideale per la pavimentazione. A differenza della moquette, i pavimenti in legno mantengono il loro colore a lungo e possono essere facilmente puliti e mantenuti, tuttavia, essendo un materiale naturale, la maggior parte dei pavimenti in legno richiede l&#039;applicazione di una finitura superficiale per proteggere il legno da vari tipi di danni come graffi e graffi. scheggiature nel tempo. In questo studio, una Nanovea <a href=\"https:\/\/nanovea.com\/tribometers\/\">Tribometro<\/a> \u00e8 stato utilizzato per misurare il tasso di usura e il coefficiente di attrito (COF) per comprendere meglio le prestazioni comparative di tre finiture del legno.<\/p>\n<p>Il comportamento in servizio di una specie legnosa utilizzata per la pavimentazione \u00e8 spesso correlato alla sua resistenza all'usura. La variazione della struttura cellulare e fibrosa delle diverse specie di legno contribuisce al loro diverso comportamento meccanico e tribologico. I test di servizio reali sul legno come materiale per pavimentazione sono costosi, difficili da riprodurre e richiedono lunghi periodi di prova. Di conseguenza, diventa importante sviluppare un semplice test di usura che possa produrre risultati affidabili, riproducibili e immediati.<\/p>\n\n<p style=\"text-align: left; color: #1b96cf; font-size: 24px;\">Obiettivo di misurazione<\/p>\n<p>In questo studio abbiamo simulato e confrontato il comportamento all'usura di tre tipi di legno per dimostrare la capacit\u00e0 del Tribometro Nanovea di valutare le propriet\u00e0 tribologiche del legno in modo controllato e monitorato.<\/p>\n<div style=\"text-align: center;\"><a href=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/05\/Measurement-Objective.png\"><img fetchpriority=\"high\" decoding=\"async\" class=\"alignnone size-full wp-image-8406\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/05\/Measurement-Objective.png\" alt=\"\" width=\"860\" height=\"372\"><\/a><\/div>\n<p style=\"text-align: left; color: #1b96cf; font-size: 24px;\">Discussione <strong><u><i><br><\/i><\/u><\/strong><\/p>\n<p>Descrizione del campione: Il legno duro di betulla antica ha una finitura all'ossido di alluminio a 7 strati, che protegge dall'usura quotidiana. Courtship Grey Oak e Santos Mahogany sono entrambi tipi di pavimenti laminati che variano per finitura superficiale e lucentezza. Il Courtship Grey Oak \u00e8 di colore grigio ardesia, con finitura EIR e bassa lucentezza. Il Santos Mahogany, invece, \u00e8 di colore bordeaux scuro, prefinito e ad alta lucentezza, il che consente di nascondere pi\u00f9 facilmente graffi e difetti superficiali.<\/p>\n<p>L'evoluzione della COF durante le prove di usura dei tre campioni di pavimentazione in legno \u00e8 rappresentata nella Fig. 1. I campioni Antique Birch Hardwood, Courtship Grey Oak e Santos Mahogany hanno mostrato un comportamento COF diverso.<\/p>\n<p><a href=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/05\/Evolution-of-COF.png\"><img decoding=\"async\" class=\"alignnone size-full wp-image-8407\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/05\/Evolution-of-COF.png\" alt=\"\" width=\"1280\" height=\"567\"><\/a><\/p>\n<p style=\"margin: 0in; margin-bottom: .0001pt;\"><span style=\"font-family: 'Arial',sans-serif;\">Nel grafico precedente si pu\u00f2 osservare che il legno di latifoglie di betulla antica \u00e8 stato l'unico campione a dimostrare un COF costante per tutta la durata del test. Il forte aumento del COF del Courtship Grey Oak e la successiva graduale diminuzione potrebbero indicare che la rugosit\u00e0 superficiale del campione ha contribuito in larga misura al suo comportamento COF. Con l'usura del campione, la rugosit\u00e0 della superficie \u00e8 diminuita ed \u00e8 diventata pi\u00f9 omogenea, il che spiega la diminuzione del COF quando la superficie del campione \u00e8 diventata pi\u00f9 liscia a causa dell'usura meccanica. Il COF del Santos Mahogany mostra un aumento graduale e regolare del COF all'inizio della prova, per poi passare bruscamente a un andamento discontinuo del COF. Ci\u00f2 potrebbe indicare che una volta che il rivestimento del laminato ha iniziato a consumarsi, la sfera d'acciaio (materiale di contrasto) \u00e8 entrata in contatto con il substrato di legno che si \u00e8 consumato in modo pi\u00f9 rapido e turbolento, creando un comportamento COF pi\u00f9 rumoroso verso la fine del test. <\/span><\/p>\n<p style=\"margin: 0in; margin-bottom: .0001pt;\"><span style=\"font-family: 'Arial',sans-serif; color: #1c1e29;\">&nbsp;<\/span><\/p>\n<p><a href=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/05\/Table-1-2.png\"><img decoding=\"async\" class=\"alignnone size-full wp-image-8408\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/05\/Table-1-2.png\" alt=\"\" width=\"849\" height=\"349\"><\/a><\/p>\n<p><a href=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/05\/Sample-of-Antique-Birch.jpg\"><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-8409\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/05\/Sample-of-Antique-Birch.jpg\" alt=\"\" width=\"1286\" height=\"552\"><\/a><\/p>\n<p><em><strong>Legno duro di betulla antica:<\/strong><\/em><\/p>\n<p><a href=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/05\/Figure-2-and-3-1.png\"><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-8410\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/05\/Figure-2-and-3-1.png\" alt=\"\" width=\"900\" height=\"861\"><\/a><\/p>\n\n<p><em><strong>Corteggiamento della quercia grigia:<\/strong><\/em><\/p>\n<p><a href=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/05\/Figure-4-and-Figure-5-1.png\"><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-8411\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/05\/Figure-4-and-Figure-5-1.png\" alt=\"\" width=\"895\" height=\"888\"><\/a><\/p>\n<p><em><strong>Mogano Santos<\/strong><\/em><\/p>\n<p><a href=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/05\/Figure-6-and-Figure-7-1.png\"><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-8412\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/05\/Figure-6-and-Figure-7-1.png\" alt=\"\" width=\"904\" height=\"899\"><\/a><\/p>\n<p>La Tabella 2 riassume i risultati delle scansioni e delle analisi delle tracce di usura su tutti i campioni di pavimentazione in legno dopo l'esecuzione dei test di usura. Le informazioni dettagliate e le immagini di ciascun campione sono riportate nelle Figure 2-7. Dal confronto del tasso di usura tra i tre campioni, si pu\u00f2 dedurre che il mogano Santos si \u00e8 dimostrato meno resistente all'usura meccanica rispetto agli altri due campioni. Il legno di latifoglie di betulla antica e la quercia grigia di corteggiamento hanno presentato tassi di usura molto simili, sebbene il loro comportamento durante i test differisca in modo significativo. L'Antique Birch Hardwood ha avuto un andamento graduale e pi\u00f9 uniforme dell'usura, mentre il Court-ship Grey Oak ha mostrato una traccia di usura poco profonda e bucherellata, dovuta alla struttura e alla finitura superficiale preesistente.<\/p>\n<p><a href=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/05\/Table-2.png\"><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-8413\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/05\/Table-2.png\" alt=\"\" width=\"855\" height=\"214\"><\/a><\/p>\n<p style=\"text-align: left; color: #1b96cf; font-size: 24px;\">Conclusione<\/p>\n\n<p><a href=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/05\/Conclusion-1.jpg\"><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-8414\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/05\/Conclusion-1.jpg\" alt=\"\" width=\"930\" height=\"539\"><\/a><\/p>\n\n<p>In questo studio abbiamo dimostrato la capacit\u00e0 del Tribometro Nanovea di valutare il coefficiente di attrito e la resistenza all'usura di tre tipi di legno, il legno duro di betulla antica, la quercia grigia di corteggiamento e il mogano Santos, in modo controllato e monitorato. Le propriet\u00e0 meccaniche superiori del legno duro di betulla antica ne determinano una migliore resistenza all'usura. La struttura e l'omogeneit\u00e0 della superficie del legno svolgono un ruolo importante nel comportamento all'usura. La struttura superficiale del Rovere grigio Courtship, come gli spazi vuoti o le fessure tra le fibre cellulari del legno, possono diventare i punti deboli in cui l'usura ha inizio e si propaga.<\/p>\n\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-8eff728 elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"8eff728\" data-element_type=\"section\" data-settings=\"{&quot;background_background&quot;:&quot;classic&quot;}\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-2288b64\" data-id=\"2288b64\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-f5503cb elementor-widget elementor-widget-heading\" data-id=\"f5503cb\" data-element_type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\"><b>PARLIAMO ORA DELLA VOSTRA APPLICAZIONE<\/b><\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-1d97879 live-chat elementor-align-center elementor-widget elementor-widget-button\" data-id=\"1d97879\" data-element_type=\"widget\" data-widget_type=\"button.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<div class=\"elementor-button-wrapper\">\n\t\t\t\t\t<a class=\"elementor-button elementor-button-link elementor-size-md\" href=\"https:\/\/nanovea.com\/contact\/live-chat\/\" id=\"live-chat\">\n\t\t\t\t\t\t<span class=\"elementor-button-content-wrapper\">\n\t\t\t\t\t\t\t\t\t<span class=\"elementor-button-text\">CHAT IN DIRETTA<\/span>\n\t\t\t\t\t<\/span>\n\t\t\t\t\t<\/a>\n\t\t\t\t<\/div>\n\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<\/div>","protected":false},"excerpt":{"rendered":"<p>Importance of Comparing Wood Finish Wear &amp; COF Wood has been used for thousands of years as a building material for homes, furniture, and flooring. It has a combination of natural beauty, and durability, making it an ideal candidate for flooring. Unlike carpet, hardwood floors keep their color for a long time and can be [&hellip;]<\/p>","protected":false},"author":1,"featured_media":8417,"comment_status":"open","ping_status":"open","sticky":false,"template":"","format":"standard","meta":{"_exactmetrics_skip_tracking":false,"_exactmetrics_sitenote_active":false,"_exactmetrics_sitenote_note":"","_exactmetrics_sitenote_category":0,"footnotes":""},"categories":[7,349,351,353,355,335,373,336],"tags":[],"class_list":["post-8403","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-application-notes","category-laboratory-testing","category-profilometry-roughness-finish","category-profilometry-texture-grain","category-profilometry-volume-area","category-profilometry-testing","category-rotational-tribology","category-tribology-testing"],"_links":{"self":[{"href":"https:\/\/nanovea.com\/it\/wp-json\/wp\/v2\/posts\/8403","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/nanovea.com\/it\/wp-json\/wp\/v2\/posts"}],"about":[{"href":"https:\/\/nanovea.com\/it\/wp-json\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"https:\/\/nanovea.com\/it\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/nanovea.com\/it\/wp-json\/wp\/v2\/comments?post=8403"}],"version-history":[{"count":15,"href":"https:\/\/nanovea.com\/it\/wp-json\/wp\/v2\/posts\/8403\/revisions"}],"predecessor-version":[{"id":23433,"href":"https:\/\/nanovea.com\/it\/wp-json\/wp\/v2\/posts\/8403\/revisions\/23433"}],"wp:featuredmedia":[{"embeddable":true,"href":"https:\/\/nanovea.com\/it\/wp-json\/wp\/v2\/media\/8417"}],"wp:attachment":[{"href":"https:\/\/nanovea.com\/it\/wp-json\/wp\/v2\/media?parent=8403"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"https:\/\/nanovea.com\/it\/wp-json\/wp\/v2\/categories?post=8403"},{"taxonomy":"post_tag","embeddable":true,"href":"https:\/\/nanovea.com\/it\/wp-json\/wp\/v2\/tags?post=8403"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}