{"id":8370,"date":"2020-05-11T16:08:36","date_gmt":"2020-05-11T16:08:36","guid":{"rendered":"https:\/\/nanovea.com\/?p=8370"},"modified":"2023-11-13T23:23:08","modified_gmt":"2023-11-13T23:23:08","slug":"microindentazione-frattura-di-roccia-minerale","status":"publish","type":"post","link":"https:\/\/nanovea.com\/it\/microindentazione-frattura-di-roccia-minerale\/","title":{"rendered":"Migliorare le procedure di estrazione con la microindicazione"},"content":{"rendered":"<div data-elementor-type=\"wp-post\" data-elementor-id=\"8370\" class=\"elementor elementor-8370\" data-elementor-post-type=\"post\">\n\t\t\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-2ac048 elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"2ac048\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-4549d56f\" data-id=\"4549d56f\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-77bd32bb elementor-widget elementor-widget-text-editor\" data-id=\"77bd32bb\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p style=\"text-align: left; color: #1b96cf; font-size: 24px;\"><strong><em>RICERCA SULLA MICROINDENTAZIONE E CONTROLLO DI QUALIT\u00c0<\/em><u><i><br><\/i><\/u><\/strong><\/p>\n<p>La meccanica delle rocce \u00e8 lo studio del comportamento meccanico delle masse rocciose e trova applicazione nei settori dell'estrazione mineraria, della perforazione, della produzione di giacimenti e delle costruzioni civili. La strumentazione avanzata, che consente di misurare con precisione le propriet\u00e0 meccaniche, permette di migliorare i pezzi e le procedure in questi settori. Il successo delle procedure di controllo della qualit\u00e0 \u00e8 garantito dalla comprensione della meccanica delle rocce a livello microscopico.<\/p>\n<div><a href=\"https:\/\/nanovea.com\/micro-indentation-tester\/\">Microindentazione<\/a> \u00e8 uno strumento fondamentale utilizzato per gli studi relativi alla meccanica delle rocce. Queste tecniche fanno progredire le tecniche di scavo, fornendo un'ulteriore comprensione delle propriet\u00e0 della massa rocciosa. La microindentazione viene utilizzata per migliorare le teste di perforazione e quindi le procedure di estrazione. La microindentazione \u00e8 stata utilizzata per studiare la formazione di gesso e polvere dai minerali. Gli studi di microindentazione possono includere durezza, modulo di Young, creep, stress-strain, tenacit\u00e0 alla frattura e compressione con un unico strumento.<\/div>\n<div>&nbsp;<\/div>\n<div>&nbsp;<\/div>\n<p style=\"text-align: left; color: #1b96cf; font-size: 24px;\"><em><strong>OBIETTIVO DI MISURAZIONE<\/strong><\/em><\/p>\n<p>In questa applicazione la Nanovea <a href=\"https:\/\/nanovea.com\/mechanical-testers\/\">tester meccanico<\/a> misura la durezza Vickers (Hv), il modulo di Young e la resistenza alla frattura di un campione di roccia minerale. La roccia \u00e8 costituita da biotite, feldspato e quarzo che formano il composito standard del granito. Ciascuno viene testato separatamente.<\/p>\n<div style=\"text-align: center;\"><a href=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/05\/Sample-of-Rock.png\"><img fetchpriority=\"high\" decoding=\"async\" class=\"alignnone size-full wp-image-8382\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/05\/Sample-of-Rock.png\" alt=\"\" width=\"899\" height=\"880\"><\/a><\/div>\n<div style=\"text-align: center;\">&nbsp;<\/div>\n<p style=\"text-align: left; color: #1b96cf; font-size: 24px;\"><em><strong>RISULTATI E DISCUSSIONE<\/strong><\/em><u><i><\/i><\/u><\/p>\n<p style=\"margin: 0in; margin-bottom: .0001pt;\"><span style=\"font-family: 'Arial',sans-serif;\">Questa sezione comprende una tabella riassuntiva che confronta i principali risultati numerici per i diversi campioni, seguita dall'elenco completo dei risultati, che include ogni indentazione eseguita, accompagnata dalle micrografie dell'indentazione, quando disponibili. Questi risultati completi presentano i valori misurati di durezza e modulo di Young e la profondit\u00e0 di penetrazione (\u0394d) con le loro medie e deviazioni standard. Si deve considerare che una grande variazione nei risultati pu\u00f2 verificarsi nel caso in cui la rugosit\u00e0 della superficie sia nella stessa gamma di dimensioni dell'indentazione.<\/span><\/p>\n<p style=\"margin: 0in; margin-bottom: .0001pt;\"><span style=\"font-family: 'Arial',sans-serif;\"><br>Tabella riassuntiva dei principali risultati numerici per la durezza e la tenacit\u00e0 alla frattura<\/span><\/p>\n<p style=\"margin: 0in; margin-bottom: .0001pt;\"><span style=\"font-family: 'Arial',sans-serif; color: #1c1e29;\">&nbsp;<\/span><\/p>\n<p><a href=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/05\/2-Summary-Table.png\"><img decoding=\"async\" class=\"alignnone size-full wp-image-8421\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/05\/2-Summary-Table.png\" alt=\"\" width=\"1189\" height=\"783\"><\/a><\/p>\n<p><a href=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/05\/Biotite-detailed-hardness.png\"><img decoding=\"async\" class=\"alignnone size-full wp-image-8373\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/05\/Biotite-detailed-hardness.png\" alt=\"\" width=\"1251\" height=\"825\"><\/a><\/p>\n<p><a href=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/05\/Biotite-detailed-frac-toughness.png\"><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-8372\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/05\/Biotite-detailed-frac-toughness.png\" alt=\"\" width=\"1328\" height=\"780\"><\/a><\/p>\n<p><a href=\"https:\/\/nanovea.com\/wp-content\/uploads\/2020\/05\/Feldspar-Detailed-Hardness.png\"><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-8469\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2020\/05\/Feldspar-Detailed-Hardness.png\" alt=\"\" width=\"1248\" height=\"791\"><\/a><\/p>\n<p><a href=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/05\/feldspar-frac-toughness.png\"><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-8378\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/05\/feldspar-frac-toughness.png\" alt=\"\" width=\"1354\" height=\"841\"><\/a><\/p>\n<p><a href=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/05\/Quartz-Detailed-Hardness.png\"><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-8381\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/05\/Quartz-Detailed-Hardness.png\" alt=\"\" width=\"1359\" height=\"813\"><\/a><\/p>\n<p><a href=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/05\/Quartz-Detailed-Frac-Toughness.png\"><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-8380\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/05\/Quartz-Detailed-Frac-Toughness.png\" alt=\"\" width=\"1313\" height=\"797\"><\/a><\/p>\n<p style=\"text-align: left; color: #1b96cf; font-size: 24px;\"><em><strong>CONCLUSIONE<\/strong><\/em><\/p>\n<p><a href=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/05\/Conclusion.jpg\"><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-8374\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/05\/Conclusion.jpg\" alt=\"\" width=\"933\" height=\"688\"><\/a><\/p>\n<p>Il tester meccanico Nanovea ha dimostrato riproducibilit\u00e0 e precisione dei risultati di indentazione sulla superficie dura delle rocce minerali. La durezza e il modulo di Young di ciascun materiale che compone il granito sono stati misurati direttamente dalle curve di profondit\u00e0 rispetto al carico. La superficie ruvida ha comportato l'esecuzione di prove con carichi pi\u00f9 elevati che potrebbero aver causato microfessurazioni. Le microfessurazioni spiegherebbero alcune delle variazioni osservate nelle misurazioni. Le fessure non erano percepibili attraverso l'osservazione al microscopio standard a causa della superficie ruvida del campione. Pertanto, non \u00e8 possibile calcolare i numeri tradizionali di tenacit\u00e0 alla frattura, che richiedono la misurazione della lunghezza delle cricche. Invece, abbiamo usato il sistema per rilevare l'inizio delle cricche attraverso le dislocazioni nelle curve di profondit\u00e0 rispetto al carico, aumentando i carichi.<\/p>\n<p>I carichi soglia di frattura sono stati riportati ai carichi in cui si sono verificati i cedimenti. A differenza dei test tradizionali di tenacit\u00e0 alla frattura, che misurano semplicemente la lunghezza della cricca, si ottiene un carico al quale inizia la soglia di frattura. Inoltre, l'ambiente controllato e strettamente monitorato consente di misurare la durezza come valore quantitativo per confrontare una variet\u00e0 di campioni.<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-fe963ae elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"fe963ae\" data-element_type=\"section\" data-settings=\"{&quot;background_background&quot;:&quot;classic&quot;}\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-f298cde\" data-id=\"f298cde\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-feb84be elementor-widget elementor-widget-heading\" data-id=\"feb84be\" data-element_type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\"><b>PARLIAMO ORA DELLA VOSTRA APPLICAZIONE<\/b><\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-314ba67 live-chat elementor-align-center elementor-widget elementor-widget-button\" data-id=\"314ba67\" data-element_type=\"widget\" data-widget_type=\"button.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<div class=\"elementor-button-wrapper\">\n\t\t\t\t\t<a class=\"elementor-button elementor-button-link elementor-size-md\" href=\"https:\/\/nanovea.com\/contact\/live-chat\/\" id=\"live-chat\">\n\t\t\t\t\t\t<span class=\"elementor-button-content-wrapper\">\n\t\t\t\t\t\t\t\t\t<span class=\"elementor-button-text\">CHAT IN DIRETTA<\/span>\n\t\t\t\t\t<\/span>\n\t\t\t\t\t<\/a>\n\t\t\t\t<\/div>\n\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<\/div>","protected":false},"excerpt":{"rendered":"","protected":false},"author":1,"featured_media":11681,"comment_status":"open","ping_status":"open","sticky":false,"template":"","format":"standard","meta":{"_exactmetrics_skip_tracking":false,"_exactmetrics_sitenote_active":false,"_exactmetrics_sitenote_note":"","_exactmetrics_sitenote_category":0,"footnotes":""},"categories":[7,368,338,349,337],"tags":[],"class_list":["post-8370","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-application-notes","category-indentation-fracture-toughness","category-indentation-hardness-elastic","category-laboratory-testing","category-mechanical-testing"],"_links":{"self":[{"href":"https:\/\/nanovea.com\/it\/wp-json\/wp\/v2\/posts\/8370","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/nanovea.com\/it\/wp-json\/wp\/v2\/posts"}],"about":[{"href":"https:\/\/nanovea.com\/it\/wp-json\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"https:\/\/nanovea.com\/it\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/nanovea.com\/it\/wp-json\/wp\/v2\/comments?post=8370"}],"version-history":[{"count":30,"href":"https:\/\/nanovea.com\/it\/wp-json\/wp\/v2\/posts\/8370\/revisions"}],"predecessor-version":[{"id":23477,"href":"https:\/\/nanovea.com\/it\/wp-json\/wp\/v2\/posts\/8370\/revisions\/23477"}],"wp:featuredmedia":[{"embeddable":true,"href":"https:\/\/nanovea.com\/it\/wp-json\/wp\/v2\/media\/11681"}],"wp:attachment":[{"href":"https:\/\/nanovea.com\/it\/wp-json\/wp\/v2\/media?parent=8370"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"https:\/\/nanovea.com\/it\/wp-json\/wp\/v2\/categories?post=8370"},{"taxonomy":"post_tag","embeddable":true,"href":"https:\/\/nanovea.com\/it\/wp-json\/wp\/v2\/tags?post=8370"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}