{"id":4454,"date":"2019-03-11T06:06:56","date_gmt":"2019-03-11T06:06:56","guid":{"rendered":"https:\/\/nanovea.com\/?p=4454"},"modified":"2023-11-13T23:39:13","modified_gmt":"2023-11-13T23:39:13","slug":"analisi-viscoelastica-della-gomma","status":"publish","type":"post","link":"https:\/\/nanovea.com\/it\/viscoelastic-analysis-of-rubber\/","title":{"rendered":"Analisi viscoelastica della gomma"},"content":{"rendered":"<div data-elementor-type=\"wp-post\" data-elementor-id=\"4454\" class=\"elementor elementor-4454\" data-elementor-post-type=\"post\">\n\t\t\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-62b1054 elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"62b1054\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-b60b89b\" data-id=\"b60b89b\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-f4024e4 elementor-widget elementor-widget-text-editor\" data-id=\"f4024e4\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p>Analisi viscoelastica della gomma<\/p><p>Per saperne di pi\u00f9<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-2d6b9de elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"2d6b9de\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-ac59e37\" data-id=\"ac59e37\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<section class=\"elementor-section elementor-inner-section elementor-element elementor-element-d19140a elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"d19140a\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-inner-column elementor-element elementor-element-876145f\" data-id=\"876145f\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-8e5163b elementor-widget elementor-widget-spacer\" data-id=\"8e5163b\" data-element_type=\"widget\" data-widget_type=\"spacer.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t<div class=\"elementor-spacer\">\n\t\t\t<div class=\"elementor-spacer-inner\"><\/div>\n\t\t<\/div>\n\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-inner-column elementor-element elementor-element-1c69642\" data-id=\"1c69642\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-ceaea63 elementor-widget elementor-widget-html\" data-id=\"ceaea63\" data-element_type=\"widget\" data-widget_type=\"html.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<div><\/div>\r\n<a href=\"http:\/\/nanovea.com\/App-Notes\/nanoindentation-dma.pdf\"\" target=\"_blank\">\r\n<div class=\"product-features-icon-image-containter-brochure-button\">\r\n\r\n<img decoding=\"async\" class=\"alignright\" style=\"width: 200px;\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2020\/06\/DOWNLOAD-PDF-BUTTON-A-s.png\" \/>\r\n<div class=\"overlay-button\"><img decoding=\"async\" class=\"alignright\" style=\"width: 200px;\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2020\/06\/DOWNLOAD-PDF-BUTTON-B-s.png\" \/><\/div>\r\n<\/div>\r\n<\/a>\r\n<div>\u00a0<\/div>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-258d660b elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"258d660b\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-644880d7\" data-id=\"644880d7\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-7adccbda elementor-widget elementor-widget-text-editor\" data-id=\"7adccbda\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p>I pneumatici sono soggetti a deformazioni cicliche elevate quando i veicoli circolano su strada. Quando sono esposti a condizioni stradali difficili, la durata degli pneumatici \u00e8 compromessa da molti fattori, come l'usura del filo, il calore generato dall'attrito, l'invecchiamento della gomma e altri.<\/p><p>Di conseguenza, i pneumatici presentano solitamente strutture a strati compositi in gomma caricata con carbonio, corde di nylon e fili d'acciaio, ecc. In particolare, la composizione della gomma nelle diverse aree dei sistemi di pneumatici \u00e8 ottimizzata per fornire diverse propriet\u00e0 funzionali, tra cui, a titolo esemplificativo, il filo resistente all'usura, lo strato di gomma ammortizzante e lo strato di base in gomma dura.<\/p><p>Un test affidabile e ripetibile del comportamento viscoelastico della gomma \u00e8 fondamentale nel controllo di qualit\u00e0 e nella ricerca e sviluppo di nuovi pneumatici, nonch\u00e9 nella valutazione della durata di vita dei vecchi pneumatici. Analisi Dinamico-Meccanica (DMA) durante <a href=\"https:\/\/nanovea.com\/nano-indentation-tester\/\">Nanoindentazione <\/a>\u00e8 una tecnica per caratterizzare la viscoelasticit\u00e0. Quando viene applicata una sollecitazione oscillatoria controllata, viene misurata la deformazione risultante, consentendo agli utenti di determinare il modulo complesso dei materiali testati.<\/p><p><a href=\"http:\/\/nanovea.com\/App-Notes\/nanoindentation-dma.pdf\"><img fetchpriority=\"high\" decoding=\"async\" class=\"alignnone wp-image-4463\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2019\/03\/Tire-cover.jpg\" alt=\"\" width=\"316\" height=\"403\" \/><\/a><\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<\/div>","protected":false},"excerpt":{"rendered":"<p>Analisi viscoelastica della gomma Per saperne di pi\u00f9<\/p>","protected":false},"author":1,"featured_media":4478,"comment_status":"open","ping_status":"open","sticky":false,"template":"","format":"standard","meta":{"_exactmetrics_skip_tracking":false,"_exactmetrics_sitenote_active":false,"_exactmetrics_sitenote_note":"","_exactmetrics_sitenote_category":0,"footnotes":""},"categories":[7,343,349,337,1],"tags":[],"class_list":["post-4454","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-application-notes","category-loss-storage","category-laboratory-testing","category-mechanical-testing","category-uncategorized"],"_links":{"self":[{"href":"https:\/\/nanovea.com\/it\/wp-json\/wp\/v2\/posts\/4454","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/nanovea.com\/it\/wp-json\/wp\/v2\/posts"}],"about":[{"href":"https:\/\/nanovea.com\/it\/wp-json\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"https:\/\/nanovea.com\/it\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/nanovea.com\/it\/wp-json\/wp\/v2\/comments?post=4454"}],"version-history":[{"count":16,"href":"https:\/\/nanovea.com\/it\/wp-json\/wp\/v2\/posts\/4454\/revisions"}],"predecessor-version":[{"id":23501,"href":"https:\/\/nanovea.com\/it\/wp-json\/wp\/v2\/posts\/4454\/revisions\/23501"}],"wp:featuredmedia":[{"embeddable":true,"href":"https:\/\/nanovea.com\/it\/wp-json\/wp\/v2\/media\/4478"}],"wp:attachment":[{"href":"https:\/\/nanovea.com\/it\/wp-json\/wp\/v2\/media?parent=4454"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"https:\/\/nanovea.com\/it\/wp-json\/wp\/v2\/categories?post=4454"},{"taxonomy":"post_tag","embeddable":true,"href":"https:\/\/nanovea.com\/it\/wp-json\/wp\/v2\/tags?post=4454"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}