{"id":8403,"date":"2019-05-12T13:32:24","date_gmt":"2019-05-12T13:32:24","guid":{"rendered":"https:\/\/nanovea.com\/?p=8403"},"modified":"2023-11-13T22:38:12","modified_gmt":"2023-11-13T22:38:12","slug":"holz-verschleis-test-mit-dem-nanovea-tribometer","status":"publish","type":"post","link":"https:\/\/nanovea.com\/de\/wood-wear-test-with-the-nanovea-tribometer\/","title":{"rendered":"Holzverschlei\u00dftest mit dem Nanovea Tribometer"},"content":{"rendered":"<div data-elementor-type=\"wp-post\" data-elementor-id=\"8403\" class=\"elementor elementor-8403\" data-elementor-post-type=\"post\">\n\t\t\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-3127429d elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"3127429d\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-4aead9d\" data-id=\"4aead9d\" data-element_type=\"column\" data-settings=\"{&quot;background_background&quot;:&quot;classic&quot;}\">\n\t\t\t<div class=\"elementor-widget-wrap\">\n\t\t\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-482f6253 elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"482f6253\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-270b5199\" data-id=\"270b5199\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-3131792c elementor-widget elementor-widget-text-editor\" data-id=\"3131792c\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p style=\"text-align: left; color: #1b96cf; font-size: 24px;\">Die Bedeutung des Vergleichs von Holzverschlei\u00df und COF<strong><u><i><br><\/i><\/u><\/strong><\/p>\n<p>Holz wird seit Jahrtausenden als Baumaterial f\u00fcr H\u00e4user, M\u00f6bel und Fu\u00dfb\u00f6den verwendet. Es verf\u00fcgt \u00fcber eine Kombination aus nat\u00fcrlicher Sch\u00f6nheit und Haltbarkeit, was es zu einem idealen Kandidaten f\u00fcr Bodenbel\u00e4ge macht. Im Gegensatz zu Teppichen behalten Hartholzb\u00f6den ihre Farbe lange und lassen sich leicht reinigen und pflegen. Da es sich jedoch um ein nat\u00fcrliches Material handelt, ist bei den meisten Holzb\u00f6den eine Oberfl\u00e4chenbehandlung erforderlich, um das Holz vor verschiedenen Arten von Sch\u00e4den wie Abnutzung und Abnutzung zu sch\u00fctzen splittert mit der Zeit. In dieser Studie ein Nanovea <a href=\"https:\/\/nanovea.com\/tribometers\/\">Tribometer<\/a> wurde zur Messung der Verschlei\u00dfrate und des Reibungskoeffizienten (COF) verwendet, um die Vergleichsleistung von drei Holzoberfl\u00e4chen besser zu verstehen.<\/p>\n<p>Das Nutzungsverhalten einer Holzart, die f\u00fcr Fu\u00dfb\u00f6den verwendet wird, h\u00e4ngt h\u00e4ufig mit ihrer Verschlei\u00dffestigkeit zusammen. Die Ver\u00e4nderungen in der individuellen Zell- und Faserstruktur der verschiedenen Holzarten tragen zu ihrem unterschiedlichen mechanischen und tribologischen Verhalten bei. Tats\u00e4chliche Gebrauchspr\u00fcfungen von Holz als Bodenbelag sind teuer, schwer zu reproduzieren und erfordern lange Pr\u00fcfzeiten. Daher ist es wichtig, einen einfachen Verschlei\u00dftest zu entwickeln, der zuverl\u00e4ssig, reproduzierbar und einfach durchzuf\u00fchren ist.<\/p>\n\n<p style=\"text-align: left; color: #1b96cf; font-size: 24px;\">Messung Zielsetzung<\/p>\n<p>In dieser Studie haben wir das Verschlei\u00dfverhalten von drei Holzarten simuliert und verglichen, um die F\u00e4higkeit des Nanovea Tribometers zu demonstrieren, die tribologischen Eigenschaften von Holz kontrolliert und \u00fcberwacht zu bewerten.<\/p>\n<div style=\"text-align: center;\"><a href=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/05\/Measurement-Objective.png\"><img fetchpriority=\"high\" decoding=\"async\" class=\"alignnone size-full wp-image-8406\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/05\/Measurement-Objective.png\" alt=\"\" width=\"860\" height=\"372\"><\/a><\/div>\n<p style=\"text-align: left; color: #1b96cf; font-size: 24px;\">Diskussion <strong><u><i><br><\/i><\/u><\/strong><\/p>\n<p>Muster Beschreibung: Antique Birch Hardwood ist mit einer 7-schichtigen Aluminiumoxid-Oberfl\u00e4che versehen, die Schutz vor t\u00e4glicher Abnutzung bietet. Courtship Grey Oak und Santos Mahogany sind beides Laminatb\u00f6den, die sich in der Oberfl\u00e4chenbeschaffenheit und im Glanz unterscheiden. Courtship Grey Oak hat eine schiefergraue Farbe, eine EIR-Oberfl\u00e4che und einen niedrigen Glanzgrad. Santos Mahagoni hingegen hat eine dunkle burgunderrote Farbe, ist vorlackiert und hochgl\u00e4nzend, wodurch Kratzer und Defekte auf der Oberfl\u00e4che leichter verborgen werden k\u00f6nnen.<\/p>\n<p>Die Entwicklung des COF-Wertes w\u00e4hrend der Abnutzungstests der drei Holzfu\u00dfbodenproben ist in Abb. 1 dargestellt. Die Proben \"Antique Birch Hardwood\", \"Courtship Grey Oak\" und \"Santos Mahogany\" zeigten alle ein unterschiedliches COF-Verhalten.<\/p>\n<p><a href=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/05\/Evolution-of-COF.png\"><img decoding=\"async\" class=\"alignnone size-full wp-image-8407\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/05\/Evolution-of-COF.png\" alt=\"\" width=\"1280\" height=\"567\"><\/a><\/p>\n<p style=\"margin: 0in; margin-bottom: .0001pt;\"><span style=\"font-family: 'Arial',sans-serif;\">Aus dem obigen Diagramm ist ersichtlich, dass das Laubholz Antique Birch die einzige Probe war, die w\u00e4hrend der gesamten Testdauer einen gleichm\u00e4\u00dfigen COF aufwies. Der starke Anstieg des COF der Eiche Courtship Grey und der anschlie\u00dfende allm\u00e4hliche R\u00fcckgang k\u00f6nnten darauf hindeuten, dass die Oberfl\u00e4chenrauhigkeit der Probe weitgehend zu ihrem COF-Verhalten beigetragen hat. Mit der Abnutzung der Probe nahm die Oberfl\u00e4chenrauheit ab und wurde homogener, was den R\u00fcckgang des COF erkl\u00e4rt, da die Oberfl\u00e4che der Probe durch die mechanische Abnutzung glatter wurde. Die COF von Santos Mahagoni zeigt zu Beginn des Tests einen gleichm\u00e4\u00dfigen, allm\u00e4hlichen Anstieg der COF und geht dann abrupt in einen abgehackten COF-Trend \u00fcber. Dies k\u00f6nnte darauf hindeuten, dass die Stahlkugel (Gegenmaterial) mit dem Holzsubstrat in Ber\u00fchrung kam, sobald die Laminatbeschichtung zu verschlei\u00dfen begann, was zu einer schnelleren und turbulenteren Abnutzung f\u00fchrte, die gegen Ende des Tests zu einem lauteren COF-Verhalten f\u00fchrte. <\/span><\/p>\n<p style=\"margin: 0in; margin-bottom: .0001pt;\"><span style=\"font-family: 'Arial',sans-serif; color: #1c1e29;\">&nbsp;<\/span><\/p>\n<p><a href=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/05\/Table-1-2.png\"><img decoding=\"async\" class=\"alignnone size-full wp-image-8408\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/05\/Table-1-2.png\" alt=\"\" width=\"849\" height=\"349\"><\/a><\/p>\n<p><a href=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/05\/Sample-of-Antique-Birch.jpg\"><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-8409\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/05\/Sample-of-Antique-Birch.jpg\" alt=\"\" width=\"1286\" height=\"552\"><\/a><\/p>\n<p><em><strong>Antikes Birken-Hartholz:<\/strong><\/em><\/p>\n<p><a href=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/05\/Figure-2-and-3-1.png\"><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-8410\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/05\/Figure-2-and-3-1.png\" alt=\"\" width=\"900\" height=\"861\"><\/a><\/p>\n\n<p><em><strong>Brautwerbung Graue Eiche:<\/strong><\/em><\/p>\n<p><a href=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/05\/Figure-4-and-Figure-5-1.png\"><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-8411\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/05\/Figure-4-and-Figure-5-1.png\" alt=\"\" width=\"895\" height=\"888\"><\/a><\/p>\n<p><em><strong>Santos Mahagoni<\/strong><\/em><\/p>\n<p><a href=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/05\/Figure-6-and-Figure-7-1.png\"><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-8412\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/05\/Figure-6-and-Figure-7-1.png\" alt=\"\" width=\"904\" height=\"899\"><\/a><\/p>\n<p>Tabelle 2 fasst die Ergebnisse der Verschlei\u00dfspuren-Scans und -Analysen aller Holzbodenproben nach der Durchf\u00fchrung der Verschlei\u00dftests zusammen. Detaillierte Informationen und Bilder f\u00fcr jede Probe sind in den Abbildungen 2-7 zu sehen. Aus dem Vergleich der Abnutzungsraten aller drei Proben l\u00e4sst sich ableiten, dass sich Santos Mahagoni als weniger widerstandsf\u00e4hig gegen\u00fcber mechanischer Abnutzung erweist als die beiden anderen Proben. Antique Birch Hardwood und Courtship Grey Oak hatten sehr \u00e4hnliche Abnutzungsraten, obwohl sich ihr Abnutzungsverhalten w\u00e4hrend der Tests deutlich unterschied. Antikes Birken-Laubholz wies einen allm\u00e4hlichen und gleichm\u00e4\u00dfigeren Abnutzungstrend auf, w\u00e4hrend Eiche Courtship Grey aufgrund der bereits vorhandenen Oberfl\u00e4chentextur und -behandlung eine flache und l\u00f6chrige Abnutzungsspur zeigte.<\/p>\n<p><a href=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/05\/Table-2.png\"><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-8413\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/05\/Table-2.png\" alt=\"\" width=\"855\" height=\"214\"><\/a><\/p>\n<p style=\"text-align: left; color: #1b96cf; font-size: 24px;\">Schlussfolgerung<\/p>\n\n<p><a href=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/05\/Conclusion-1.jpg\"><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-8414\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/05\/Conclusion-1.jpg\" alt=\"\" width=\"930\" height=\"539\"><\/a><\/p>\n\n<p>In dieser Studie haben wir die Leistungsf\u00e4higkeit des Tribometers von Nanovea bei der kontrollierten und \u00fcberwachten Bewertung des Reibungskoeffizienten und der Verschlei\u00dffestigkeit der drei Holzarten Antikes Birken-Hartholz, Graue Eiche und Santos-Mahagoni unter Beweis gestellt. Die \u00fcberlegenen mechanischen Eigenschaften des antiken Birken-Hartholzes f\u00fchren zu seiner besseren Verschlei\u00dffestigkeit. Die Textur und Homogenit\u00e4t der Holzoberfl\u00e4che spielen eine wichtige Rolle f\u00fcr das Verschlei\u00dfverhalten. Die Oberfl\u00e4chentextur von Courtship Grey Oak, wie z. B. L\u00fccken oder Risse zwischen den Zellfasern des Holzes, k\u00f6nnen zu Schwachstellen werden, an denen der Verschlei\u00df einsetzt und sich ausbreitet.<\/p>\n\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-8eff728 elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"8eff728\" data-element_type=\"section\" data-settings=\"{&quot;background_background&quot;:&quot;classic&quot;}\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-2288b64\" data-id=\"2288b64\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-f5503cb elementor-widget elementor-widget-heading\" data-id=\"f5503cb\" data-element_type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\"><b>UND NUN ZU IHRER BEWERBUNG<\/b><\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-1d97879 live-chat elementor-align-center elementor-widget elementor-widget-button\" data-id=\"1d97879\" data-element_type=\"widget\" data-widget_type=\"button.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<div class=\"elementor-button-wrapper\">\n\t\t\t\t\t<a class=\"elementor-button elementor-button-link elementor-size-md\" href=\"https:\/\/nanovea.com\/contact\/live-chat\/\" id=\"live-chat\">\n\t\t\t\t\t\t<span class=\"elementor-button-content-wrapper\">\n\t\t\t\t\t\t\t\t\t<span class=\"elementor-button-text\">LIVE CHAT<\/span>\n\t\t\t\t\t<\/span>\n\t\t\t\t\t<\/a>\n\t\t\t\t<\/div>\n\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<\/div>","protected":false},"excerpt":{"rendered":"<p>Importance of Comparing Wood Finish Wear &amp; COF Wood has been used for thousands of years as a building material for homes, furniture, and flooring. It has a combination of natural beauty, and durability, making it an ideal candidate for flooring. Unlike carpet, hardwood floors keep their color for a long time and can be [&hellip;]<\/p>\n","protected":false},"author":1,"featured_media":8417,"comment_status":"open","ping_status":"open","sticky":false,"template":"","format":"standard","meta":{"_exactmetrics_skip_tracking":false,"_exactmetrics_sitenote_active":false,"_exactmetrics_sitenote_note":"","_exactmetrics_sitenote_category":0,"footnotes":""},"categories":[7,349,351,353,355,335,373,336],"tags":[],"class_list":["post-8403","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-application-notes","category-laboratory-testing","category-profilometry-roughness-finish","category-profilometry-texture-grain","category-profilometry-volume-area","category-profilometry-testing","category-rotational-tribology","category-tribology-testing"],"_links":{"self":[{"href":"https:\/\/nanovea.com\/de\/wp-json\/wp\/v2\/posts\/8403","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/nanovea.com\/de\/wp-json\/wp\/v2\/posts"}],"about":[{"href":"https:\/\/nanovea.com\/de\/wp-json\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"https:\/\/nanovea.com\/de\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/nanovea.com\/de\/wp-json\/wp\/v2\/comments?post=8403"}],"version-history":[{"count":15,"href":"https:\/\/nanovea.com\/de\/wp-json\/wp\/v2\/posts\/8403\/revisions"}],"predecessor-version":[{"id":23433,"href":"https:\/\/nanovea.com\/de\/wp-json\/wp\/v2\/posts\/8403\/revisions\/23433"}],"wp:featuredmedia":[{"embeddable":true,"href":"https:\/\/nanovea.com\/de\/wp-json\/wp\/v2\/media\/8417"}],"wp:attachment":[{"href":"https:\/\/nanovea.com\/de\/wp-json\/wp\/v2\/media?parent=8403"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"https:\/\/nanovea.com\/de\/wp-json\/wp\/v2\/categories?post=8403"},{"taxonomy":"post_tag","embeddable":true,"href":"https:\/\/nanovea.com\/de\/wp-json\/wp\/v2\/tags?post=8403"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}