{"id":7991,"date":"2020-03-11T14:06:56","date_gmt":"2020-03-11T14:06:56","guid":{"rendered":"https:\/\/nanovea.com\/?p=7991"},"modified":"2025-05-22T20:55:47","modified_gmt":"2025-05-22T20:55:47","slug":"ertrag-und-festigkeit-von-stahl-und-aluminium","status":"publish","type":"post","link":"https:\/\/nanovea.com\/de\/yield-and-tensile-strength-of-steel-and-aluminum\/","title":{"rendered":"Streckgrenze und Zugfestigkeit von Stahl und Aluminium"},"content":{"rendered":"<div data-elementor-type=\"wp-post\" data-elementor-id=\"7991\" class=\"elementor elementor-7991\" data-elementor-post-type=\"post\">\n\t\t\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-1ec8323 elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"1ec8323\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-9ffd566\" data-id=\"9ffd566\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-a82aa85 elementor-widget elementor-widget-heading\" data-id=\"a82aa85\" data-element_type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\">Bedeutung der Messung der Streckgrenze und der Zugfestigkeit mit Hilfe der Eindr\u00fcckung<\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-47a219fe elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"47a219fe\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-a791500\" data-id=\"a791500\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-29485db5 elementor-widget elementor-widget-text-editor\" data-id=\"29485db5\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p>Traditionell werden Streckgrenze und Zugfestigkeit mit einer gro\u00dfen Zugpr\u00fcfmaschine gepr\u00fcft, die eine enorme Kraft ben\u00f6tigt, um die Proben auseinander zu ziehen. Es ist kostspielig und zeitaufw\u00e4ndig, viele Testkupons f\u00fcr ein Material zu bearbeiten, bei dem jede Probe nur einmal gepr\u00fcft werden kann. Kleine Defekte in der Probe f\u00fchren zu einer deutlichen Abweichung der Pr\u00fcfergebnisse. Unterschiedliche Konfigurationen und Ausrichtungen der auf dem Markt befindlichen Zugpr\u00fcfger\u00e4te f\u00fchren oft zu erheblichen Abweichungen in der Pr\u00fcfmechanik und den Ergebnissen.<\/p>\n<div>Die innovative Eindringmethode von Nanovea liefert direkt Werte f\u00fcr die Streckgrenze und die Zugfestigkeit, die mit den Werten vergleichbar sind, die mit herk\u00f6mmlichen Zugtests gemessen werden. Diese Messung er\u00f6ffnet neue Pr\u00fcfm\u00f6glichkeiten f\u00fcr alle Branchen. Der einfache Versuchsaufbau reduziert die Zeit und die Kosten f\u00fcr die Probenvorbereitung im Vergleich zur komplexen Couponform, die f\u00fcr Zugversuche erforderlich ist, erheblich. Mehrere Messungen an einer einzigen Probe sind bei einer geringen Gr\u00f6\u00dfe der Vertiefung m\u00f6glich. Sie verhindert den Einfluss von Defekten, die bei der Bearbeitung von Zugproben entstehen. YS- und UTS-Messungen an kleinen Proben in einem begrenzten Bereich erm\u00f6glichen die Kartierung und Erkennung lokaler Defekte in Rohrleitungen oder Autostrukturen.<\/div>\n<div>&nbsp;<\/div>\n<div>&nbsp;<\/div>\n<p style=\"text-align: left; color: #1b96cf; font-size: 24px;\">Messung Zielsetzung<\/p>\n<p>Bei dieser Anwendung wird das Nanovea <a href=\"https:\/\/nanovea.com\/mechanical-testers\/\">Mechanischer Tester<\/a> Misst die Streckgrenze und Zugfestigkeit von Proben aus Edelstahl SS304 und Aluminium Al6061-Metalllegierungen. Die Proben wurden aufgrund ihrer allgemein anerkannten Streckgrenzen- und Zugfestigkeitswerte ausgew\u00e4hlt, die die Zuverl\u00e4ssigkeit der Eindruckmethoden von Nanovea belegen.<\/p>\n<div style=\"text-align: center;\"><a href=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/03\/Measurement-Objective.png\"><img fetchpriority=\"high\" decoding=\"async\" class=\"alignnone size-full wp-image-7998\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/03\/Measurement-Objective.png\" alt=\"\" width=\"754\" height=\"453\"><\/a><\/div>\n<p style=\"text-align: left; color: #1b96cf; font-size: 24px;\">Testverfahren und -abl\u00e4ufe<strong><u><i><br><\/i><\/u><\/strong><\/p>\n<p>Die Pr\u00fcfungen der Streckgrenze und der Zugfestigkeit wurden mit dem Nanovea-Mechanik-Testger\u00e4t in der <a href=\"https:\/\/nanovea.com\/micro-indentation-tester\/\">Mikroindentation<\/a> Modus. F\u00fcr diese Anwendung wurde eine zylindrische flache Diamantspitze mit einem Durchmesser von 200 \u03bcm verwendet. Die Legierungen SS304 und Al6061 wurden aufgrund ihrer umfangreichen industriellen Anwendung und ihrer allgemein anerkannten Werte f\u00fcr die Streckgrenze und die Zugfestigkeit ausgew\u00e4hlt, um das gro\u00dfe Potenzial und die Zuverl\u00e4ssigkeit der Eindringmethode zu zeigen. Die Proben wurden vor der Pr\u00fcfung mechanisch auf Hochglanz poliert, um eine Beeinflussung der Pr\u00fcfergebnisse durch Oberfl\u00e4chenrauhigkeit oder -fehler zu vermeiden. Die Pr\u00fcfbedingungen sind in Tabelle 1 aufgef\u00fchrt. An jeder Probe wurden mehr als zehn Pr\u00fcfungen durchgef\u00fchrt, um die Wiederholbarkeit der Pr\u00fcfwerte zu gew\u00e4hrleisten.<\/p>\n<div style=\"text-align: center;\"><a href=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/03\/Table-1-1.png\"><img decoding=\"async\" class=\"size-full wp-image-7994 aligncenter\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/03\/Table-1-1.png\" alt=\"\" width=\"717\" height=\"314\"><\/a><\/div>\n<p style=\"text-align: left; color: #1b96cf; font-size: 24px;\">Ergebnisse und Diskussion<u><i><\/i><\/u><\/p>\n<p style=\"margin: 0in; margin-bottom: .0001pt;\"><span style=\"font-family: 'Arial',sans-serif;\">Die Kraft-Weg-Kurven der SS304- und Al6061-Legierungsproben sind in Abbildung 3 dargestellt, wobei die Abdr\u00fccke der flachen Eindringk\u00f6rper auf den Testproben eingezeichnet sind. Die Analyse der \"S\"-f\u00f6rmigen Belastungskurve mit Hilfe spezieller, von Nanovea entwickelter Algorithmen berechnet die Streckgrenze und die Zugfestigkeit. Die Werte werden von der Software automatisch berechnet und sind in Tabelle 1 zusammengefasst. Zum Vergleich sind die Werte f\u00fcr die Streckgrenze und die Zugfestigkeit aufgef\u00fchrt, die mit herk\u00f6mmlichen Zugversuchen ermittelt wurden.<\/span><\/p>\n<p style=\"margin: 0in; margin-bottom: .0001pt;\"><span style=\"font-family: 'Arial',sans-serif; color: #1c1e29;\">&nbsp;<\/span><\/p>\n<p><a href=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/03\/Figure-2-and-Table-2.png\"><img decoding=\"async\" class=\"alignnone size-full wp-image-7995\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/03\/Figure-2-and-Table-2.png\" alt=\"\" width=\"876\" height=\"808\"><\/a><\/p>\n<p style=\"text-align: left; color: #1b96cf; font-size: 24px;\">Schlussfolgerung<\/p>\n<p><a href=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/03\/Mech-Conclusion-photo.png\"><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-7997\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2017\/03\/Mech-Conclusion-photo.png\" alt=\"\" width=\"1150\" height=\"536\"><\/a><\/p>\n<p>In dieser Studie haben wir die Leistungsf\u00e4higkeit des Nanovea Mechanical Tester bei der Bewertung der Streckgrenze und Zugfestigkeit von Blechproben aus rostfreiem Stahl und Aluminiumlegierungen demonstriert. Der einfache Versuchsaufbau reduziert den Zeit- und Kostenaufwand f\u00fcr die Probenvorbereitung f\u00fcr Zugversuche erheblich. Die kleine Vertiefungsgr\u00f6\u00dfe erm\u00f6glicht die Durchf\u00fchrung mehrerer Messungen an einer einzigen Probe. Diese Methode erm\u00f6glicht YS\/UTS-Messungen an kleinen Proben und lokalisierten Bereichen und bietet eine L\u00f6sung f\u00fcr die YS\/UTS-Kartierung und lokale Defekterkennung von Rohrleitungen oder Autostrukturen.<\/p>\n<p>Die Nano-, Mikro- oder Makromodule des Nanovea Mechanical Tester umfassen alle ISO- und ASTM-konforme Eindring-, Kratz- und Verschlei\u00dftestmodi und bieten so das umfassendste und benutzerfreundlichste Testspektrum, das in einem einzigen System verf\u00fcgbar ist. Das un\u00fcbertroffene Sortiment von Nanovea ist eine ideale L\u00f6sung zur Bestimmung des gesamten Spektrums mechanischer Eigenschaften d\u00fcnner oder dicker, weicher oder harter Beschichtungen, Filme und Substrate, einschlie\u00dflich H\u00e4rte, Elastizit\u00e4tsmodul, Bruchz\u00e4higkeit, Haftung, Verschlei\u00dffestigkeit und vielen anderen. Dar\u00fcber hinaus sind ein optionaler ber\u00fchrungsloser 3D-Profiler und ein AFM-Modul f\u00fcr die hochaufl\u00f6sende 3D-Bildgebung von Eindr\u00fccken, Kratzern und Verschlei\u00dfspuren zus\u00e4tzlich zu anderen Oberfl\u00e4chenmessungen wie Rauheit erh\u00e4ltlich.<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-d6b5798 elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"d6b5798\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-f4bf8f7\" data-id=\"f4bf8f7\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-be15913 elementor-widget elementor-widget-heading\" data-id=\"be15913\" data-element_type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\">Haben Sie eine \u00e4hnliche Anwendung?<\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-4ddfda0 elementor-align-justify open-chat elementor-widget elementor-widget-button\" data-id=\"4ddfda0\" data-element_type=\"widget\" data-widget_type=\"button.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<div class=\"elementor-button-wrapper\">\n\t\t\t\t\t<a class=\"elementor-button elementor-size-sm\" role=\"button\">\n\t\t\t\t\t\t<span class=\"elementor-button-content-wrapper\">\n\t\t\t\t\t\t\t\t\t<span class=\"elementor-button-text\">JETZT MIT EINEM EXPERTEN DISKUTIEREN<\/span>\n\t\t\t\t\t<\/span>\n\t\t\t\t\t<\/a>\n\t\t\t\t<\/div>\n\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-c1b8ee6 elementor-align-justify button-quote elementor-widget elementor-widget-button\" data-id=\"c1b8ee6\" data-element_type=\"widget\" data-widget_type=\"button.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<div class=\"elementor-button-wrapper\">\n\t\t\t\t\t<a class=\"elementor-button elementor-button-link elementor-size-sm\" href=\"https:\/\/nanovea.com\/contact-sales-form\/\" id=\"button-quote-bottom\">\n\t\t\t\t\t\t<span class=\"elementor-button-content-wrapper\">\n\t\t\t\t\t\t\t\t\t<span class=\"elementor-button-text\">PREISE UND DETAILS SCHNELL ERHALTEN<\/span>\n\t\t\t\t\t<\/span>\n\t\t\t\t\t<\/a>\n\t\t\t\t<\/div>\n\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<\/div>","protected":false},"excerpt":{"rendered":"","protected":false},"author":1,"featured_media":11691,"comment_status":"open","ping_status":"open","sticky":false,"template":"","format":"standard","meta":{"_exactmetrics_skip_tracking":false,"_exactmetrics_sitenote_active":false,"_exactmetrics_sitenote_note":"","_exactmetrics_sitenote_category":0,"footnotes":""},"categories":[7,344,349,337],"tags":[],"class_list":["post-7991","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-application-notes","category-indentation-yield-strength-fatigue","category-laboratory-testing","category-mechanical-testing"],"_links":{"self":[{"href":"https:\/\/nanovea.com\/de\/wp-json\/wp\/v2\/posts\/7991","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/nanovea.com\/de\/wp-json\/wp\/v2\/posts"}],"about":[{"href":"https:\/\/nanovea.com\/de\/wp-json\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"https:\/\/nanovea.com\/de\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/nanovea.com\/de\/wp-json\/wp\/v2\/comments?post=7991"}],"version-history":[{"count":34,"href":"https:\/\/nanovea.com\/de\/wp-json\/wp\/v2\/posts\/7991\/revisions"}],"predecessor-version":[{"id":24782,"href":"https:\/\/nanovea.com\/de\/wp-json\/wp\/v2\/posts\/7991\/revisions\/24782"}],"wp:featuredmedia":[{"embeddable":true,"href":"https:\/\/nanovea.com\/de\/wp-json\/wp\/v2\/media\/11691"}],"wp:attachment":[{"href":"https:\/\/nanovea.com\/de\/wp-json\/wp\/v2\/media?parent=7991"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"https:\/\/nanovea.com\/de\/wp-json\/wp\/v2\/categories?post=7991"},{"taxonomy":"post_tag","embeddable":true,"href":"https:\/\/nanovea.com\/de\/wp-json\/wp\/v2\/tags?post=7991"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}