{"id":6927,"date":"2019-09-04T16:59:53","date_gmt":"2019-09-04T16:59:53","guid":{"rendered":"https:\/\/nanovea.com\/?p=6927"},"modified":"2023-11-13T22:37:18","modified_gmt":"2023-11-13T22:37:18","slug":"schmier-augen-tropfen-vergleich-mit-dem-nanovea-t50-tribometer","status":"publish","type":"post","link":"https:\/\/nanovea.com\/de\/lubricating-eye-drop-comparison-using-the-nanovea-t50-tribometer\/","title":{"rendered":"Vergleich von schmierenden Augentropfen mit dem Tribometer Nanovea T50"},"content":{"rendered":"<div data-elementor-type=\"wp-post\" data-elementor-id=\"6927\" class=\"elementor elementor-6927\" data-elementor-post-type=\"post\">\n\t\t\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-21cd638d elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"21cd638d\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-42ec104d\" data-id=\"42ec104d\" data-element_type=\"column\" data-settings=\"{&quot;background_background&quot;:&quot;classic&quot;}\">\n\t\t\t<div class=\"elementor-widget-wrap\">\n\t\t\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-42d11421 elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"42d11421\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-55297c0c\" data-id=\"55297c0c\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-6ba397b8 elementor-widget elementor-widget-text-editor\" data-id=\"6ba397b8\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p style=\"text-align: left; color: #1b96cf; font-size: 24px;\">Bedeutung der Pr\u00fcfung von Augentropfenl\u00f6sungen<strong><u><i><br><\/i><\/u><\/strong><\/p>\n<div>Augentropfen werden zur Linderung von Symptomen eingesetzt, die durch eine Reihe von Augenproblemen verursacht werden. So k\u00f6nnen sie beispielsweise zur Behandlung kleinerer Augenreizungen (z. B. Trockenheit und R\u00f6tung), zur Verz\u00f6gerung des Auftretens eines Glaukoms oder zur Behandlung von Infektionen eingesetzt werden. Freiverk\u00e4ufliche Augentropfen werden haupts\u00e4chlich zur Behandlung von Trockenheit eingesetzt. Ihre Wirksamkeit bei der Befeuchtung des Auges kann mit einem Reibungskoeffiziententest verglichen und gemessen werden.<\/div>\n<div>&nbsp;<\/div>\n<div>Trockene Augen k\u00f6nnen durch eine Vielzahl von Faktoren verursacht werden, z. B. durch \u00dcberanstrengung der Augen am Computer oder durch Aufenthalt im Freien bei extremen Wetterbedingungen. Gute feuchtigkeitsspendende Augentropfen tragen dazu bei, die Feuchtigkeit auf der Au\u00dfenfl\u00e4che der Augen zu erhalten und zu erg\u00e4nzen. Dadurch werden die mit trockenen Augen verbundenen Beschwerden wie Brennen, Reizung und R\u00f6tung gelindert. Durch die Messung des Reibungskoeffizienten (COF) einer Augentropfenl\u00f6sung l\u00e4sst sich ihre Schmierwirkung ermitteln und mit anderen L\u00f6sungen vergleichen.<\/div>\n\n<p style=\"text-align: left; color: #1b96cf; font-size: 24px;\">Messung Zielsetzung<\/p>\n<p>In dieser Studie wurde der Reibungskoeffizient (COF) von drei verschiedenen schmierenden Augentropfenl\u00f6sungen mit Hilfe des Stift-auf-Scheibe-Aufbaus auf dem Nanovea T50 Tribometer gemessen.<\/p>\n<div style=\"text-align: center;\"><a href=\"https:\/\/nanovea.com\/wp-content\/uploads\/2019\/09\/Measurement-objective-picture.png\"><img fetchpriority=\"high\" decoding=\"async\" class=\"alignnone size-full wp-image-8113\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2019\/09\/Measurement-objective-picture.png\" alt=\"\" width=\"917\" height=\"649\"><\/a><\/div>\n<p style=\"text-align: left; color: #1b96cf; font-size: 24px;\">Testverfahren und -abl\u00e4ufe<strong><u><i><br><\/i><\/u><\/strong><\/p>\n<p>Ein kugelf\u00f6rmiger Stift aus Aluminiumoxid mit einem Durchmesser von 6 mm wurde auf einem Glasobjekttr\u00e4ger angebracht, wobei jede Augentropfenl\u00f6sung als Schmiermittel zwischen den beiden Oberfl\u00e4chen diente. Die f\u00fcr alle Experimente verwendeten Testparameter sind in Tabelle 1 zusammengefasst.<\/p>\n<div style=\"text-align: center;\"><a href=\"https:\/\/nanovea.com\/wp-content\/uploads\/2019\/09\/Samples-picture.png\"><img decoding=\"async\" class=\"alignnone size-full wp-image-8114\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2019\/09\/Samples-picture.png\" alt=\"\" width=\"604\" height=\"805\"><\/a><\/div>\n<p style=\"text-align: left; color: #1b96cf; font-size: 24px;\">Ergebnisse und Diskussion<u><i><\/i><\/u><\/p>\n<p style=\"margin: 0in; margin-bottom: .0001pt;\"><span style=\"font-family: 'Arial',sans-serif;\">Die Maximal-, Minimal- und Durchschnittswerte des Reibungskoeffizienten f\u00fcr die drei getesteten Augentropfenl\u00f6sungen sind in der folgenden Tabelle 2 aufgef\u00fchrt. Die Diagramme COF gegen Umdrehungen f\u00fcr jede Augentropfenl\u00f6sung sind in den Abbildungen 2-4 dargestellt. Der Reibungskoeffizient blieb bei jedem Test w\u00e4hrend des gr\u00f6\u00dften Teils der gesamten Testdauer relativ konstant. Probe A hatte den niedrigsten durchschnittlichen COF, was darauf hindeutet, dass sie die besten Schmiereigenschaften aufwies.<\/span><\/p>\n<p style=\"margin: 0in; margin-bottom: .0001pt;\"><span style=\"font-family: 'Arial',sans-serif; color: #1c1e29;\">&nbsp;<\/span><\/p>\n<p><a href=\"https:\/\/nanovea.com\/wp-content\/uploads\/2019\/09\/Figure-2.png\"><img decoding=\"async\" class=\"alignnone size-full wp-image-8115\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2019\/09\/Figure-2.png\" alt=\"\" width=\"1001\" height=\"893\"><\/a><\/p>\n<p><a href=\"https:\/\/nanovea.com\/wp-content\/uploads\/2019\/09\/Figure-3.png\"><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-8116\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2019\/09\/Figure-3.png\" alt=\"\" width=\"1285\" height=\"776\"><\/a><\/p>\n<p><a href=\"https:\/\/nanovea.com\/wp-content\/uploads\/2019\/09\/Figure-4.png\"><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-8117\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2019\/09\/Figure-4.png\" alt=\"\" width=\"1267\" height=\"794\"><\/a><\/p>\n<p style=\"text-align: left; color: #1b96cf; font-size: 24px;\">Schlussfolgerung<\/p>\n<p><a href=\"https:\/\/nanovea.com\/wp-content\/uploads\/2019\/09\/CoefficientofFrictionofEyeDrop.jpg\"><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-8121\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2019\/09\/CoefficientofFrictionofEyeDrop.jpg\" alt=\"\" width=\"1216\" height=\"777\"><\/a><\/p>\n<p>In dieser Studie zeigen wir die F\u00e4higkeit des Nanovea T50 Tribometers, den Reibungskoeffizienten von drei Augentropfenl\u00f6sungen zu messen. Anhand dieser Werte zeigen wir, dass Probe A einen niedrigeren Reibungskoeffizienten hat und daher im Vergleich zu den anderen beiden Proben eine bessere Schmierung aufweist.<\/p>\n<p>Nanovea <a href=\"https:\/\/nanovea.com\/tribometers\/\">Tribometer <\/a>bietet pr\u00e4zise und wiederholbare Verschlei\u00df- und Reibungstests mit ISO- und ASTM-konformen Rotations- und Linearmodulen. Es bietet au\u00dferdem optionale Hochtemperatur-Verschlei\u00df-, Schmier- und Tribokorrosionsmodule, die in einem vorintegrierten System verf\u00fcgbar sind. Diese Vielseitigkeit erm\u00f6glicht es Benutzern, die reale Anwendungsumgebung besser zu simulieren und das grundlegende Verst\u00e4ndnis des Verschlei\u00dfmechanismus und der tribologischen Eigenschaften verschiedener Materialien zu verbessern.<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-2f41878 elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"2f41878\" data-element_type=\"section\" data-settings=\"{&quot;background_background&quot;:&quot;classic&quot;}\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-a6030dc\" data-id=\"a6030dc\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-acb17e4 elementor-widget elementor-widget-heading\" data-id=\"acb17e4\" data-element_type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\"><b>UND NUN ZU IHRER BEWERBUNG<\/b><\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-f96103e live-chat elementor-align-center elementor-widget elementor-widget-button\" data-id=\"f96103e\" data-element_type=\"widget\" data-widget_type=\"button.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<div class=\"elementor-button-wrapper\">\n\t\t\t\t\t<a class=\"elementor-button elementor-button-link elementor-size-md\" href=\"https:\/\/nanovea.com\/contact\/live-chat\/\" id=\"live-chat\">\n\t\t\t\t\t\t<span class=\"elementor-button-content-wrapper\">\n\t\t\t\t\t\t\t\t\t<span class=\"elementor-button-text\">LIVE CHAT<\/span>\n\t\t\t\t\t<\/span>\n\t\t\t\t\t<\/a>\n\t\t\t\t<\/div>\n\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<\/div>","protected":false},"excerpt":{"rendered":"<p>Importance of Testing Eye Drop Solutions Eye drop solutions are used to alleviate symptoms caused by a range of eye problems. For example, they can be used to treat minor eye irritation (e.g. dryness and redness), delay the onset of glaucoma or treat infections. Eye drop solutions sold over-the-counter are mainly used to treat dryness. [&hellip;]<\/p>\n","protected":false},"author":1,"featured_media":6936,"comment_status":"open","ping_status":"open","sticky":false,"template":"","format":"standard","meta":{"_exactmetrics_skip_tracking":false,"_exactmetrics_sitenote_active":false,"_exactmetrics_sitenote_note":"","_exactmetrics_sitenote_category":0,"footnotes":""},"categories":[7,349,380,373,336],"tags":[],"class_list":["post-6927","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-application-notes","category-laboratory-testing","category-liquid-tribology","category-rotational-tribology","category-tribology-testing"],"_links":{"self":[{"href":"https:\/\/nanovea.com\/de\/wp-json\/wp\/v2\/posts\/6927","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/nanovea.com\/de\/wp-json\/wp\/v2\/posts"}],"about":[{"href":"https:\/\/nanovea.com\/de\/wp-json\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"https:\/\/nanovea.com\/de\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/nanovea.com\/de\/wp-json\/wp\/v2\/comments?post=6927"}],"version-history":[{"count":17,"href":"https:\/\/nanovea.com\/de\/wp-json\/wp\/v2\/posts\/6927\/revisions"}],"predecessor-version":[{"id":23430,"href":"https:\/\/nanovea.com\/de\/wp-json\/wp\/v2\/posts\/6927\/revisions\/23430"}],"wp:featuredmedia":[{"embeddable":true,"href":"https:\/\/nanovea.com\/de\/wp-json\/wp\/v2\/media\/6936"}],"wp:attachment":[{"href":"https:\/\/nanovea.com\/de\/wp-json\/wp\/v2\/media?parent=6927"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"https:\/\/nanovea.com\/de\/wp-json\/wp\/v2\/categories?post=6927"},{"taxonomy":"post_tag","embeddable":true,"href":"https:\/\/nanovea.com\/de\/wp-json\/wp\/v2\/tags?post=6927"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}