{"id":10619,"date":"2021-02-25T22:49:17","date_gmt":"2021-02-25T22:49:17","guid":{"rendered":"https:\/\/nanovea.com\/?p=10619"},"modified":"2025-09-09T22:59:34","modified_gmt":"2025-09-09T22:59:34","slug":"reifenprofiltiefenmessung","status":"publish","type":"post","link":"https:\/\/nanovea.com\/de\/tire-tread-depth-measurement\/","title":{"rendered":"Messung der Reifenprofiltiefe und der Rauheit der Gummioberfl\u00e4che | 3D-Optischer Profiler"},"content":{"rendered":"<div data-elementor-type=\"wp-post\" data-elementor-id=\"10619\" class=\"elementor elementor-10619\" data-elementor-post-type=\"post\">\n\t\t\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-cf7b158 elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"cf7b158\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-0b246ca\" data-id=\"0b246ca\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-9c8dd15 elementor-widget elementor-widget-text-editor\" data-id=\"9c8dd15\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<h1 style=\"text-align: center; font-style: italic; font-weight: bold; line-height: 1.4;\"><span style=\"font-size: 40px; color: #1b96cf; display: block;\">MESSUNG DER REIFENPROFILTIEFE UND DER RAUHIGKEIT DER GUMMIOBERFL\u00c4CHE\n<\/span><span style=\"font-size: 32px; color: #000;\">Verwendung eines optischen 3D-Profilmessger\u00e4ts\n<\/span><\/h1>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-8992fa5 elementor-widget elementor-widget-image\" data-id=\"8992fa5\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img fetchpriority=\"high\" decoding=\"async\" width=\"1024\" height=\"290\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2021\/02\/Rubber-Tread-Contour-Measurement-NANOVEA-Profilometer.jpg\" class=\"attachment-large size-large wp-image-10633\" alt=\"Referenz zur Messung der Reifenprofiltiefe mit mehreren Autoreifenprofilen\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-a98eab3 elementor-widget elementor-widget-heading\" data-id=\"a98eab3\" data-element_type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\">Vorbereitet von<\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-fade1fb elementor-widget elementor-widget-heading\" data-id=\"fade1fb\" data-element_type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\">ANDREA HERRMANN<\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-afb1e21 elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"afb1e21\" data-element_type=\"section\" data-settings=\"{&quot;background_background&quot;:&quot;gradient&quot;}\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-cd8f487\" data-id=\"cd8f487\" data-element_type=\"column\" data-settings=\"{&quot;background_background&quot;:&quot;gradient&quot;}\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-1c870be elementor-widget elementor-widget-text-editor\" data-id=\"1c870be\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\tW\u00e4hrend die Profiltiefe von Reifen zur Sicherheit der Verbraucher \u00fcblicherweise mit Handmessger\u00e4ten gemessen wird, ben\u00f6tigen industrielle Forschungs- und Entwicklungsabteilungen sowie Reifenhersteller fortschrittlichere Methoden. Diese Anwendungsbeschreibung zeigt, wie ein optisches 3D-Profilometer pr\u00e4zise Messungen der Profiltiefe, Konturkartierungen und Analysen der Rauheit der Gummioberfl\u00e4che f\u00fcr hochgenaue Untersuchungen erm\u00f6glicht.\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<section class=\"elementor-section elementor-inner-section elementor-element elementor-element-a714598 elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"a714598\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-inner-column elementor-element elementor-element-83c4e7d\" data-id=\"83c4e7d\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-6b957c1 elementor-widget elementor-widget-heading\" data-id=\"6b957c1\" data-element_type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\">EINF\u00dcHRUNG<\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-9bcf924 elementor-widget elementor-widget-text-editor\" data-id=\"9bcf924\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\tWie bei allen Materialien h\u00e4ngt auch der Reibungskoeffizient von Gummi zum Teil von seiner Oberfl\u00e4chenrauheit ab. Bei Fahrzeugreifen wirken sich sowohl die Profiltiefe als auch die Oberfl\u00e4chenrauheit direkt auf die Traktion, das Bremsverhalten und den Verschlei\u00df aus. In dieser Studie werden die Rauheit und die Abmessungen der Gummioberfl\u00e4che und des Profils mithilfe einer ber\u00fchrungslosen 3D-Profilometrie analysiert.\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-d1e69fd elementor-widget elementor-widget-image\" data-id=\"d1e69fd\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img decoding=\"async\" width=\"806\" height=\"625\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2021\/02\/Rubber-Surface-Roughness-Profilometry.png\" class=\"attachment-large size-large wp-image-10622\" alt=\"Reifenprobe zur Messung der Profiltiefe und der Rauheit der Gummioberfl\u00e4che\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-b384831 elementor-widget elementor-widget-text-editor\" data-id=\"b384831\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p>DIE PROBE<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-4ff6101 elementor-widget elementor-widget-text-editor\" data-id=\"4ff6101\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p>BEDEUTUNG DER BER\u00dcHRUNGSLOSEN 3D-PROFILOMETRIE F\u00dcR DIE MESSUNG DER REIFENPROFILTIEFE<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-747b80c elementor-widget elementor-widget-text-editor\" data-id=\"747b80c\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p>Im Gegensatz zu anderen Techniken wie Tastk\u00f6pfen oder Interferometrie, <a href=\"https:\/\/nanovea.com\/profilometers\/\">Die ber\u00fchrungslosen 3D-Optikprofiler von NANOVEA<\/a> Verwenden Sie den axialen Chromatismus, um nahezu jede Oberfl\u00e4che zu messen.<\/p><p>Das offene Staging-System des Profilers erm\u00f6glicht eine Vielzahl von Probengr\u00f6\u00dfen und erfordert keinerlei Probenvorbereitung. Mit einem einzigen Scan k\u00f6nnen Benutzer sowohl die gesamte Profiltiefe des Reifens als auch die Oberfl\u00e4chenrauheit auf Mikroebene erfassen, ohne dass die Reflektivit\u00e4t oder Absorption der Probe einen Einfluss hat. Dar\u00fcber hinaus verf\u00fcgen diese Profiler \u00fcber die fortschrittliche F\u00e4higkeit, hohe Oberfl\u00e4chenwinkel zu messen, ohne dass die Ergebnisse softwarem\u00e4\u00dfig manipuliert werden m\u00fcssen.<\/p><p>Diese Vielseitigkeit macht die Profilermessger\u00e4te von NANOVEA ideal sowohl f\u00fcr die Pr\u00fcfung des Reifenprofils als auch f\u00fcr die fortgeschrittene Forschung im Bereich Gummimaterialien.<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-193bee4 elementor-reverse-mobile elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"193bee4\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-cfd6558\" data-id=\"cfd6558\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-30070fc elementor-widget elementor-widget-heading\" data-id=\"30070fc\" data-element_type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\">MESSZIEL<\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-0e99f1e elementor-widget elementor-widget-text-editor\" data-id=\"0e99f1e\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p>In dieser Anwendung zeigen wir Ihnen die <a href=\"https:\/\/nanovea.com\/instruments\/st400\/\">NANOVEA ST400<\/a>, ein ber\u00fchrungsloses 3D-Optikprofilometer, das die Profiltiefe, Konturgeometrie und Oberfl\u00e4chenrauheit von Reifen misst. F\u00fcr diese Studie wurde nach dem Zufallsprinzip eine Probefl\u00e4che ausgew\u00e4hlt, die gro\u00df genug war, um die gesamte Reifenoberfl\u00e4che zu repr\u00e4sentieren. Zur Quantifizierung der Eigenschaften des Gummis haben wir die Analysesoftware NANOVEA Ultra 3D verwendet, um die Abmessungen der Rillen, die Profiltiefe, die Oberfl\u00e4chenrauheit und die entwickelte Fl\u00e4che im Vergleich zur projizierten Fl\u00e4che zu messen.<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<section class=\"elementor-section elementor-inner-section elementor-element elementor-element-63de4cb elementor-reverse-mobile elementor-section-full_width elementor-reverse-tablet elementor-section-height-default elementor-section-height-default\" data-id=\"63de4cb\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-no\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-inner-column elementor-element elementor-element-fd78032\" data-id=\"fd78032\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-8ed0d82 elementor-widget elementor-widget-text-editor\" data-id=\"8ed0d82\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p style=\"text-align: center; font-size: 20pt; color: black;\">NANOVEA <span style=\"font-size: 20pt; color: #1b96cf;\">ST400 Standard<\/span><br \/>Optisches 3D-Profilometer<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t<div class=\"elementor-element elementor-element-6a78543 e-grid e-con-full e-con e-child\" data-id=\"6a78543\" data-element_type=\"container\">\n\t\t\t\t<div class=\"elementor-element elementor-element-35a54da elementor-align-center homepage-button-brochure elementor-widget elementor-widget-button\" data-id=\"35a54da\" data-element_type=\"widget\" data-widget_type=\"button.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<div class=\"elementor-button-wrapper\">\n\t\t\t\t\t<a class=\"elementor-button elementor-button-link elementor-size-sm\" href=\"https:\/\/nanovea.com\/st400-profilometer-brochure-form\/\" id=\"homepage-button-brochure\">\n\t\t\t\t\t\t<span class=\"elementor-button-content-wrapper\">\n\t\t\t\t\t\t\t\t\t<span class=\"elementor-button-text\">BROSCH\u00dcRE HERUNTERLADEN<\/span>\n\t\t\t\t\t<\/span>\n\t\t\t\t\t<\/a>\n\t\t\t\t<\/div>\n\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-6874866 elementor-align-center homepage-button-quote elementor-widget elementor-widget-button\" data-id=\"6874866\" data-element_type=\"widget\" data-widget_type=\"button.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<div class=\"elementor-button-wrapper\">\n\t\t\t\t\t<a class=\"elementor-button elementor-button-link elementor-size-sm\" href=\"https:\/\/nanovea.com\/contact-sales-form\/\" id=\"homepage-button-quote\">\n\t\t\t\t\t\t<span class=\"elementor-button-content-wrapper\">\n\t\t\t\t\t\t\t\t\t<span class=\"elementor-button-text\">ANGEBOT EINHOLEN<\/span>\n\t\t\t\t\t<\/span>\n\t\t\t\t\t<\/a>\n\t\t\t\t<\/div>\n\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-inner-column elementor-element elementor-element-a156f9f\" data-id=\"a156f9f\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-4c47230 elementor-widget elementor-widget-image\" data-id=\"4c47230\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<a href=\"https:\/\/nanovea.com\/instruments\/st500\">\n\t\t\t\t\t\t\t<img decoding=\"async\" width=\"300\" height=\"296\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2020\/12\/Nanovea-Customizable-Profilometer.png\" class=\"elementor-animation-grow attachment-medium size-medium wp-image-9779\" alt=\"Nanovea ST400 3D-Optisches Profilometer zur Analyse der Profiltiefe und Oberfl\u00e4chenrauheit von Reifen\" \/>\t\t\t\t\t\t\t\t<\/a>\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-1ba4d91 elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"1ba4d91\" data-element_type=\"section\" data-settings=\"{&quot;background_background&quot;:&quot;classic&quot;}\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-45a6719\" data-id=\"45a6719\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-c95d832 elementor-widget elementor-widget-text-editor\" data-id=\"c95d832\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<span class=\"fontstyle0\" style=\"color: #1b96cf;\">ANALYSE: <\/span><span class=\"fontstyle0\" style=\"color: #ffffff;\">REIFENFADEN<\/span>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-8cd344f elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"8cd344f\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-aca91ad\" data-id=\"aca91ad\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-d6a303e elementor-widget elementor-widget-text-editor\" data-id=\"d6a303e\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\tDie 3D-Ansicht und die Falschfarbenansicht der Lauffl\u00e4chen zeigen den Wert der Kartierung von 3D-Oberfl\u00e4chendesigns. Dies bietet Ingenieuren ein einfaches Werkzeug, um die Gleichm\u00e4\u00dfigkeit der Profiltiefe, das Rillendesign und den Verschlei\u00df aus verschiedenen Blickwinkeln zu bewerten. Die erweiterte Konturanalyse und die Stufenh\u00f6henanalyse sind beide \u00e4u\u00dferst leistungsstarke Werkzeuge zur pr\u00e4zisen Messung der Abmessungen von Musterformen und -designs.\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-f5f5811 elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"f5f5811\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-top-column elementor-element elementor-element-6ee2929\" data-id=\"6ee2929\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-87f2429 elementor-widget elementor-widget-image\" data-id=\"87f2429\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img loading=\"lazy\" decoding=\"async\" width=\"512\" height=\"426\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2021\/02\/Rubber-Tire-Tread-Scan-Profilometer.jpg\" class=\"attachment-large size-large wp-image-10627\" alt=\"Falschfarben-3D-Optische Profilometrie der Reifenprofiltiefe und Rillengeometrie\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-8949fb3 elementor-widget elementor-widget-image\" data-id=\"8949fb3\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img loading=\"lazy\" decoding=\"async\" width=\"592\" height=\"397\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2021\/02\/Rubber-Tyre-3D-Scan-Profilometer.jpg\" class=\"attachment-large size-large wp-image-10629\" alt=\"3D-Profilometer-Oberfl\u00e4chenansicht der Reifenprofiltiefenmessung\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-top-column elementor-element elementor-element-58032d8\" data-id=\"58032d8\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-874e994 elementor-widget elementor-widget-text-editor\" data-id=\"874e994\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p><span class=\"fontstyle0\">ERWEITERTE KONTURANALYSE<\/span><\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-97d4ed4 elementor-widget elementor-widget-image\" data-id=\"97d4ed4\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img loading=\"lazy\" decoding=\"async\" width=\"879\" height=\"744\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2021\/02\/Rubber-Tire-Tread-Contour-Analysis.jpg\" class=\"attachment-large size-large wp-image-10626\" alt=\"Erweiterte Konturanalyse von Reifenprofilrillen mittels 3D-Profilometrie\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-16b45c6 elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"16b45c6\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-cd02096\" data-id=\"cd02096\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-bbd3cac elementor-widget elementor-widget-spacer\" data-id=\"bbd3cac\" data-element_type=\"widget\" data-widget_type=\"spacer.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t<div class=\"elementor-spacer\">\n\t\t\t<div class=\"elementor-spacer-inner\"><\/div>\n\t\t<\/div>\n\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-69527ee elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"69527ee\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-808400d\" data-id=\"808400d\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-ac2dcc8 elementor-widget elementor-widget-text-editor\" data-id=\"ac2dcc8\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p><span class=\"fontstyle0\">STUFENH\u00d6HENANALYSE<\/span> <\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-74c284d elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"74c284d\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-774c7c1\" data-id=\"774c7c1\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<section class=\"elementor-section elementor-inner-section elementor-element elementor-element-adf4c7c elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"adf4c7c\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-inner-column elementor-element elementor-element-a3e4bd6\" data-id=\"a3e4bd6\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap\">\n\t\t\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-inner-column elementor-element elementor-element-bc1f9b6\" data-id=\"bc1f9b6\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-67300af elementor-widget elementor-widget-image\" data-id=\"67300af\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img loading=\"lazy\" decoding=\"async\" width=\"761\" height=\"126\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2021\/02\/Rubber-Tire-Step-Height-Analysis-Profiler.jpg\" class=\"attachment-large size-large wp-image-10625\" alt=\"\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<div class=\"elementor-element elementor-element-c9edc39 elementor-widget elementor-widget-image\" data-id=\"c9edc39\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img loading=\"lazy\" decoding=\"async\" width=\"1024\" height=\"255\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2021\/02\/Rubber-Tire-Step-Height-Analysis-by-NANOVEA.jpg\" class=\"attachment-large size-large wp-image-10624\" alt=\"Stufenh\u00f6henanalyse zur Messung der Reifenprofiltiefe mit einem optischen 3D-Profiler\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<section class=\"elementor-section elementor-inner-section elementor-element elementor-element-cd48d19 elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"cd48d19\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-inner-column elementor-element elementor-element-26c6154\" data-id=\"26c6154\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap\">\n\t\t\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-inner-column elementor-element elementor-element-68bda50\" data-id=\"68bda50\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-319a2af elementor-widget elementor-widget-image\" data-id=\"319a2af\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img loading=\"lazy\" decoding=\"async\" width=\"513\" height=\"124\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2021\/02\/Rubber-Tire-Step-Height-Analysis-by-NANOVEA-Profilometer.jpg\" class=\"attachment-large size-large wp-image-10623\" alt=\"\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<div class=\"elementor-element elementor-element-bb09da1 elementor-widget elementor-widget-image\" data-id=\"bb09da1\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img loading=\"lazy\" decoding=\"async\" width=\"1024\" height=\"256\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2021\/02\/Rubber-Tyre-Step-Height-Analysis-by-NANOVEA.jpg\" class=\"attachment-large size-large wp-image-10630\" alt=\"3D-Profilometrie-Stufenh\u00f6henprofil zur Messung der Reifenprofiltiefe\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-9d748c9 elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"9d748c9\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-4f35edb\" data-id=\"4f35edb\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-6b373f7 elementor-widget elementor-widget-spacer\" data-id=\"6b373f7\" data-element_type=\"widget\" data-widget_type=\"spacer.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t<div class=\"elementor-spacer\">\n\t\t\t<div class=\"elementor-spacer-inner\"><\/div>\n\t\t<\/div>\n\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-fe96b86 elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"fe96b86\" data-element_type=\"section\" data-settings=\"{&quot;background_background&quot;:&quot;classic&quot;}\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-802e0b2\" data-id=\"802e0b2\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-ab299ba elementor-widget elementor-widget-text-editor\" data-id=\"ab299ba\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<span class=\"fontstyle0\" style=\"color: #1b96cf;\">ANALYSE: <\/span><span class=\"fontstyle0\" style=\"color: #ffffff;\">GUMMI OBERFL\u00c4CHE<\/span>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-a547451 elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"a547451\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-8e08d0d\" data-id=\"8e08d0d\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-6acaf28 elementor-widget elementor-widget-text-editor\" data-id=\"6acaf28\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\tDie Gummioberfl\u00e4che kann mithilfe integrierter Softwaretools auf vielf\u00e4ltige Weise quantifiziert werden, wie in den folgenden Abbildungen dargestellt. Es ist zu erkennen, dass die Oberfl\u00e4chenrauheit 2,688 \u03bcm betr\u00e4gt und das Verh\u00e4ltnis von entwickelter Fl\u00e4che zu projizierter Fl\u00e4che 9,410 mm\u00b2 zu 8,997 mm\u00b2 betr\u00e4gt. Diese Ergebnisse zeigen, wie sich die Rauheit der Gummioberfl\u00e4che auf die Traktion und Leistung auswirkt, und erm\u00f6glichen Vergleiche zwischen verschiedenen Gummimischungen oder unterschiedlichen Abnutzungsgraden der Oberfl\u00e4che.\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-9dc9c98 elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"9dc9c98\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-top-column elementor-element elementor-element-b7d4c89\" data-id=\"b7d4c89\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-04a7201 elementor-widget elementor-widget-image\" data-id=\"04a7201\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img loading=\"lazy\" decoding=\"async\" width=\"591\" height=\"415\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2021\/02\/Tire-Rubber-Surface-Analysis-Scan-NANOVEA.jpg\" class=\"attachment-large size-large wp-image-10621\" alt=\"Analyse der Rauheit von Gummioberfl\u00e4chen mit einem optischen 3D-Profilometer\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-44b6364 elementor-widget elementor-widget-image\" data-id=\"44b6364\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img loading=\"lazy\" decoding=\"async\" width=\"610\" height=\"314\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2021\/02\/Tire-Rubber-Surface-Analysis-Scan-NANOVEA-Profilometer.jpg\" class=\"attachment-large size-large wp-image-10631\" alt=\"ISO 25178 H\u00f6henparameter der Reifengummioberfl\u00e4che\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t<div class=\"elementor-column elementor-col-50 elementor-top-column elementor-element elementor-element-74c76bf\" data-id=\"74c76bf\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-e82168a elementor-widget elementor-widget-image\" data-id=\"e82168a\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img loading=\"lazy\" decoding=\"async\" width=\"716\" height=\"505\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2021\/02\/Rubber-Tyre-Surface-Analysis-NANOVEA.jpg\" class=\"attachment-large size-large wp-image-10620\" alt=\"3D-optische Profilometrieansicht der Oberfl\u00e4chenrauheit von Gummi und der entwickelten Fl\u00e4che\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-e746e2f elementor-widget elementor-widget-image\" data-id=\"e746e2f\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img loading=\"lazy\" decoding=\"async\" width=\"610\" height=\"169\" src=\"https:\/\/nanovea.com\/wp-content\/uploads\/2021\/02\/Rubber-Tread-Contour-Measurement-NANOVEA-Profilometer-08-09-20.jpg\" class=\"attachment-large size-large wp-image-10628\" alt=\"Parameter f\u00fcr Reifengummioberfl\u00e4chenprofiler\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-3ae9e0d elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"3ae9e0d\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-d4a53b2\" data-id=\"d4a53b2\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-82b43fc elementor-widget elementor-widget-heading\" data-id=\"82b43fc\" data-element_type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\">SCHLUSSFOLGERUNG<\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-7435d64 elementor-widget elementor-widget-text-editor\" data-id=\"7435d64\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\tIn dieser Anwendung haben wir gezeigt, wie der ber\u00fchrungslose optische 3D-Profiler von NANOVEA die Profiltiefe, Konturma\u00dfe und Oberfl\u00e4chenrauheit von Reifen pr\u00e4zise charakterisieren kann. Die Daten zeigen eine Oberfl\u00e4chenrauheit von 2,69 \u00b5m und eine entwickelte Fl\u00e4che von 9,41 mm\u00b2 bei einer projizierten Fl\u00e4che von 9 mm\u00b2. Au\u00dferdem wurden verschiedene Abmessungen und Radien der Gummiprofile gemessen. Diese Informationen k\u00f6nnen von Reifenherstellern, Automobilforschern und Werkstoffingenieuren verwendet werden, um Profildesigns, Gummimischungen oder Reifen mit unterschiedlichem Verschlei\u00dfgrad zu vergleichen. Die hier gezeigten Daten stellen nur einen Teil der Berechnungen dar, die in der Ultra 3D-Analysesoftware verf\u00fcgbar sind.\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-87e6b5b elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"87e6b5b\" data-element_type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-53c5f8a\" data-id=\"53c5f8a\" data-element_type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-b11e64c elementor-widget elementor-widget-heading\" data-id=\"b11e64c\" data-element_type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\">Haben Sie eine \u00e4hnliche Anwendung?<\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-5847677 elementor-align-justify open-chat elementor-widget elementor-widget-button\" data-id=\"5847677\" data-element_type=\"widget\" data-widget_type=\"button.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<div class=\"elementor-button-wrapper\">\n\t\t\t\t\t<a class=\"elementor-button elementor-size-sm\" role=\"button\">\n\t\t\t\t\t\t<span class=\"elementor-button-content-wrapper\">\n\t\t\t\t\t\t\t\t\t<span class=\"elementor-button-text\">JETZT MIT EINEM EXPERTEN DISKUTIEREN<\/span>\n\t\t\t\t\t<\/span>\n\t\t\t\t\t<\/a>\n\t\t\t\t<\/div>\n\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-6265531 elementor-align-justify button-quote elementor-widget elementor-widget-button\" data-id=\"6265531\" data-element_type=\"widget\" data-widget_type=\"button.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<div class=\"elementor-button-wrapper\">\n\t\t\t\t\t<a class=\"elementor-button elementor-button-link elementor-size-sm\" href=\"https:\/\/nanovea.com\/contact-sales-form\/\" id=\"button-quote-bottom\">\n\t\t\t\t\t\t<span class=\"elementor-button-content-wrapper\">\n\t\t\t\t\t\t\t\t\t<span class=\"elementor-button-text\">PREISE UND DETAILS SCHNELL ERHALTEN<\/span>\n\t\t\t\t\t<\/span>\n\t\t\t\t\t<\/a>\n\t\t\t\t<\/div>\n\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<\/div>","protected":false},"excerpt":{"rendered":"<p>Learn how the Nanovea ST400 3D Optical Profiler provides precise tire tread depth measurement and rubber surface roughness analysis for tire performance and wear studies.<\/p>","protected":false},"author":1,"featured_media":10751,"comment_status":"open","ping_status":"open","sticky":false,"template":"","format":"standard","meta":{"_exactmetrics_skip_tracking":false,"_exactmetrics_sitenote_active":false,"_exactmetrics_sitenote_note":"","_exactmetrics_sitenote_category":0,"footnotes":""},"categories":[7,349,350,351,352,353,355,335],"tags":[],"class_list":["post-10619","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-application-notes","category-laboratory-testing","category-profilometry-geometry-shape","category-profilometry-roughness-finish","category-profilometry-step-height-thickness","category-profilometry-texture-grain","category-profilometry-volume-area","category-profilometry-testing"],"_links":{"self":[{"href":"https:\/\/nanovea.com\/de\/wp-json\/wp\/v2\/posts\/10619","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/nanovea.com\/de\/wp-json\/wp\/v2\/posts"}],"about":[{"href":"https:\/\/nanovea.com\/de\/wp-json\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"https:\/\/nanovea.com\/de\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/nanovea.com\/de\/wp-json\/wp\/v2\/comments?post=10619"}],"version-history":[{"count":149,"href":"https:\/\/nanovea.com\/de\/wp-json\/wp\/v2\/posts\/10619\/revisions"}],"predecessor-version":[{"id":25083,"href":"https:\/\/nanovea.com\/de\/wp-json\/wp\/v2\/posts\/10619\/revisions\/25083"}],"wp:featuredmedia":[{"embeddable":true,"href":"https:\/\/nanovea.com\/de\/wp-json\/wp\/v2\/media\/10751"}],"wp:attachment":[{"href":"https:\/\/nanovea.com\/de\/wp-json\/wp\/v2\/media?parent=10619"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"https:\/\/nanovea.com\/de\/wp-json\/wp\/v2\/categories?post=10619"},{"taxonomy":"post_tag","embeddable":true,"href":"https:\/\/nanovea.com\/de\/wp-json\/wp\/v2\/tags?post=10619"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}